Deformed steel bar with high anti-seismic property and heat treatment method thereof

Through the heat treatment process of continuous casting, two cooling and normalizing treatment on rebar, and subsequent rolling, the existing high-strength rebar lacks seismic resistance, and better tensile strength and seismic resistance are achieved. The process is simple and easy to use.

CN118932143APending Publication Date: 2024-11-12YANGJIANG ALLOY MATERIALS LAB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411058356.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The seismic resistance of existing high-strength rebar is insufficient and cannot meet the seismic resistance requirements specified in GB1499-2007.

Method used

A heat treatment method of rebar with high seismic resistance, including continuous casting, two cooling and two normalizing treatments, followed by rolling. The rebar is made to make the structure of rebar more fine and even after cooling, thereby improving resistance. Tensile strength and shock resistance.

Benefits of technology

Through this method, the tensile strength, ageing and seismic performance of rebar are improved, and the problem of low seismic performance of existing products is solved. The process is simple and does not require new equipment investment, which is suitable for widespread promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932143A_ABST
    Figure CN118932143A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of steel heat treatment, and particularly relates to high-anti-seismic-performance deformed steel bar and a heat treatment method thereof.The heat treatment method comprises the steps that target deformed steel bar is subjected to continuous casting to obtain a casting blank, the casting blank is subjected to cooling and secondary normalizing treatment, and finally a finished product is obtained through rolling. According to the method, heat treatment is carried out before rolling, and the deformed steel bar is finer and more uniform in structure after being cooled through normalizing treatment, so that the tensile strength, the timeliness and the anti-seismic property are improved, the problem that an existing product is not high in anti-seismic property is solved, the structure of the treated finished product is ferrite and pearlite, and ferrite grains are finer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of heat treatment of steel, and in particular relates to a threaded steel with high seismic resistance and a heat treatment method thereof. Background Art

[0002] Hot-rolled ribbed steel bars are referred to as rebars or rebars. Currently, the most commonly used hot-rolled ribbed steel bars are HRB400E and HRB500E. The suffix E indicates earthquake resistance. The ratio of tensile strength to yield strength is used as the basis for testing earthquake resistance. The larger the ratio, the better the earthquake resistance. GB1499-2007 stipulates that the earthquake resistance shall not be less than 1.25. The higher the strength of the rebar, the higher the earthquake resistance requirements. Therefore, it is necessary to study a heat treatment process to improve the earthquake resistance of rebar to cope with the shortcomings of the existing technology, so as to solve or alleviate the above-mentioned problem of inadequate earthquake resistance. Summary of the invention

[0003] The present invention provides a threaded steel bar with high seismic resistance and a heat treatment method thereof, so as to solve the problem that the high-strength threaded steel bar in the prior art has insufficient seismic resistance.

[0004] To achieve the above object, the present invention proposes the following technical solutions:

[0005] A heat treatment method for high seismic resistance threaded steel comprises the following steps:

[0006] Step 1, continuously casting the target threaded steel bar to obtain a cast billet;

[0007] Step 2, cooling the ingot to room temperature to obtain an ingot after the first cooling;

[0008] Step 3, normalizing the first cooled ingot to obtain the first normalized ingot;

[0009] Step 4, cooling the first normalizing treatment ingot to room temperature to obtain the second cooled ingot;

[0010] Step 5, normalizing the ingot after the second cooling to obtain the ingot after the second normalizing treatment;

[0011] Step 6, rolling the ingot after the second normalizing treatment and cooling it to room temperature to obtain a finished product.

[0012] Preferably, the mass percentage of carbon in the target threaded steel is between 0.2% and 0.25%.

[0013] Preferably, the cooling in step 2 is specifically to cool the ingot at 1-3°C / s until the ingot temperature reaches room temperature.

[0014] Preferably, the cooling in step 4 is specifically to cool the ingot after the first normalizing treatment at a rate of 1-3°C / s until the temperature of the ingot after the first normalizing treatment reaches room temperature.

[0015] Preferably, the normalizing temperature in step 3 is 800-900°C.

[0016] Preferably, the normalizing temperature in step 5 is 800-900°C.

[0017] Preferably, the cooling in step 6 is specifically to cool the rolled ingot at 1-3°C / s until the rolled ingot is cooled to room temperature.

[0018] A threaded steel bar with high seismic resistance, wherein the threaded steel bar is prepared by a heat treatment method for a threaded steel bar with high seismic resistance.

[0019] The present invention is beneficial in that:

[0020] The present invention proposes to perform heat treatment before both rolling processes, and to make the structure of the threaded steel finer and more uniform after cooling through normalizing treatment, thereby improving the tensile strength, timeliness and seismic resistance, so as to solve the problem of low seismic resistance of existing products. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:

[0022] Figure 1 A schematic diagram of a heat treatment method for threaded steel with high seismic resistance;

[0023] Figure 2 A comparison diagram of a heat treatment method process for high seismic resistance threaded steel and the original process;

[0024] Figure 3 This is a schematic diagram of the mixed crystal structure of the sample before heat treatment without modification;

[0025] Figure 4 Schematic diagram of sample organization after changing the heat treatment process. DETAILED DESCRIPTION

[0026] The present invention will be described in detail below with reference to the accompanying drawings and in combination with embodiments. It should be noted that the embodiments and features in the embodiments of the present invention can be combined with each other without conflict.

[0027] The following detailed description is an exemplary description, which is intended to provide further detailed description of the present invention. Unless otherwise specified, all technical terms used in the present invention have the same meaning as those generally understood by those skilled in the art to which the present invention belongs. The terms used in the present invention are only for describing specific embodiments, and are not intended to limit the exemplary embodiments according to the present invention.

[0028] See also Figure 1 As shown, the present invention provides a heat treatment method for threaded steel with high seismic resistance, comprising the following steps:

[0029] Step 1, continuously casting the target threaded steel bar to obtain a cast billet;

[0030] Step 2, cooling the ingot at a cooling temperature of 1-3°C / s until the temperature of the ingot reaches room temperature, thereby obtaining the ingot after the first cooling;

[0031] Step 3, normalizing the ingot after the first cooling, the temperature of the normalizing treatment is 800-900° C., to obtain the ingot after the first normalizing treatment, the internal structure of the ingot after the normalizing treatment is more refined and uniform;

[0032] Step 4, cooling the first normalizing ingot at a cooling temperature of 1-3°C / s until the temperature of the first normalizing ingot reaches room temperature, thereby obtaining the second cooled ingot;

[0033] Step 5, normalizing the ingot after the second cooling, the temperature of the normalizing treatment is 800-900° C., to obtain the ingot after the second normalizing treatment, and the internal structure of the ingot after the normalizing treatment is further refined and uniform;

[0034] Step 6, rolling and cooling the ingot after the second normalizing treatment, the cooling temperature is 1-3°C / s, to obtain a finished product.

[0035] In a specific embodiment, the mass percentage of C in the target threaded steel is between 0.2% and 0.25%.

[0036] In a specific embodiment, the cooling temperature in step 2, step 4 and step 6 is 1°C / s.

[0037] In a specific embodiment, the normalizing temperature in step 3 and step 5 is 900°C.

[0038] Embodiment 1:

[0039] The target threaded steel is heat treated using existing technology, specifically:

[0040] Step 1, continuously casting the target threaded steel bar to obtain a cast billet;

[0041] Step 2, directly rolling the ingot to obtain the ingot after the first rolling;

[0042] Step 3, cooling the first rolled ingot to room temperature to obtain the first cooled ingot;

[0043] Step 4, rolling the first cooled ingot again to obtain a second rolled ingot;

[0044] Step 5, cooling the ingot after the second rolling to obtain a finished product.

[0045] Embodiment 2:

[0046] The target threaded steel is heat treated by the method of the present invention, specifically:

[0047] Step 1, continuously casting the target threaded steel bar to obtain a cast billet;

[0048] Step 2, cooling the ingot at 1°C / s until the temperature of the ingot reaches room temperature, thereby obtaining the ingot after the first cooling;

[0049] Step 3, performing normalizing treatment at 900° C. on the first cooled ingot to obtain the first normalized ingot;

[0050] Step 4, cooling the ingot after the first normalizing treatment at 1°C / s until its temperature reaches room temperature, thereby obtaining the ingot after the second cooling;

[0051] Step 5, performing normalizing treatment at 900° C. again on the ingot after the second cooling to obtain the ingot after the second normalizing treatment;

[0052] Step 6, rolling the ingot after the second normalizing treatment and cooling it at 1°C / s to obtain a finished product.

[0053] The finished product in Example 1 is as follows Figure 3 As shown, the finished product in Example 2 is as follows Figure 4 shown.

[0054] It can be seen that after modifying the heat treatment process, the structure is also ferrite plus pearlite, and the ferrite grains are finer and more uniform; at the same time, this method does not require new equipment investment, the process is simple, and it is suitable for wide promotion.

[0055] The present invention also proposes a high-seismic performance threaded steel, which is obtained by the above-mentioned heat treatment method for the high-seismic performance threaded steel. Based on the above-mentioned heat treatment process, compared with the existing products, the high-seismic performance threaded steel proposed by the present invention has a finer and more uniform structure, and therefore has better yield strength, tensile strength, timeliness and seismic performance.

[0056] It is known from common technical knowledge that the present invention can be implemented by other embodiments that do not deviate from its spirit or essential features. Therefore, the above disclosed embodiments are only illustrative in all respects and are not exclusive. All changes within the scope of the present invention or within the scope equivalent to the present invention are included in the present invention.

[0057] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A heat treatment method for high seismic resistance threaded steel, characterized in that: The steps include: Step 1, continuously casting the target threaded steel bar to obtain a cast billet; Step 2, cooling the ingot to room temperature to obtain an ingot after the first cooling; Step 3, normalizing the first cooled ingot to obtain the first normalized ingot; Step 4, cooling the first normalizing treatment ingot to room temperature to obtain the second cooled ingot; Step 5, normalizing the ingot after the second cooling to obtain the ingot after the second normalizing treatment; Step 6, rolling the ingot after the second normalizing treatment and cooling it to room temperature to obtain a finished product.

2. A heat treatment method for high seismic resistance threaded steel according to claim 1, characterized in that: The mass percentage of carbon in the target threaded steel is between 0.2% and 0.25%.

3. A heat treatment method for high seismic resistance threaded steel according to claim 1, characterized in that: The cooling in step 2 is specifically to cool the ingot at a rate of 1-3°C / s until the ingot temperature reaches room temperature.

4. A heat treatment method for high seismic resistance threaded steel according to claim 1, characterized in that: The cooling in step 4 is specifically to cool the ingot after the first normalizing treatment at a rate of 1-3°C / s until the temperature of the ingot after the first normalizing treatment reaches room temperature.

5. The heat treatment method of high seismic resistance threaded steel according to claim 1, characterized in that: The normalizing temperature in step 3 is 800-900°C.

6. A heat treatment method for high seismic resistance threaded steel according to claim 1, characterized in that: The normalizing temperature in step 5 is 800-900°C.

7. A heat treatment method for high seismic resistance threaded steel according to claim 1, characterized in that: The cooling in step 6 is specifically to cool the rolled ingot at 1-3° C. / s until the rolled ingot is cooled to room temperature.

8. A high seismic resistance threaded steel bar, characterized in that: The threaded steel is prepared by a heat treatment method for threaded steel with high seismic resistance according to any one of claims 1 to 7.