Method for dealuminizing and refining intermediate alloy by aluminothermic process

By using an aluminum dealuminizer composed of calcium oxide, calcium fluoride and sodium chlorate in the intermediate frequency induction furnace to dealuminize the aluminum residue in the aluminum thermal intermediate alloy, the problem of aluminum residue is solved, and the aluminum content is effective Reduce and improve alloy purity, suitable for the production needs of different alloys.

CN118932174APending Publication Date: 2024-11-12METALINK SPECIAL ALLOYS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410995268.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The residual aluminum elements in intermediate alloys produced by aluminum thermal method limit their application range in high-temperature alloys, and how to effectively reduce the aluminum content has become an urgent problem.

Method used

Heat the intermediate alloy in an intermediate frequency induction furnace, add a dealuminum agent and stir. Use a dealuminum agent composed of calcium oxide, calcium fluoride and sodium chlorate to promote the dealuminum reaction through agitation of nickel rods to form a low melting point aluminum slag system , and then the slag was removed and continued to refine until the aluminum content decreased to less than 0.1%.

Benefits of technology

Effectively remove aluminum in intermediate alloys, improve the purity of the alloy, is suitable for different types of alloy production needs, and is low in cost, and does not require the use of high-value raw materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932174A_ABST
    Figure CN118932174A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of alloy smelting, and discloses an aluminothermic intermediate alloy dealumination refining method, which comprises the following steps: putting an intermediate alloy in a medium-frequency induction furnace, increasing power for heating, adding a dealumination agent after the alloy is completely molten, stirring for 3-5 minutes by using a nickel rod after adding, promoting a dealumination reaction, and refining for 3-10 minutes after the dealumination agent is completely added, and aluminum oxide slag generated by the reaction floats upwards and is combined with calcium fluoride and calcium oxide to form a slag system with a lower melting point, the slag is taken out after refining is finished, refining is continued for 2-8 minutes, and the alloy is cast into a mold to be cooled. According to the method, the residual aluminum in the intermediate alloy produced by the aluminothermic method can be effectively removed, and the aluminum content is stably reduced to be less than 0.1%. According to the method, efficient refining of the intermediate alloy is achieved, redundant aluminum is removed, meanwhile, the purity of other components of the alloy is kept, and the method is suitable for the production requirements of different kinds of alloys.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of nonferrous metallurgy, and specifically relates to a method for dealumination and refining of intermediate alloys by thermite process. Background Art

[0002] As a classic method of producing master alloys, the aluminothermic method plays an important role in industrial manufacturing. It can efficiently prepare various master alloys by optimizing the reaction formula and controlling the reaction heat and reaction rate. A certain amount of aluminum will inevitably remain in the master alloys produced by this method. However, in the field of high-temperature alloys, especially those high-temperature alloys that do not contain aluminum in the design requirements, the trace presence of aluminum may be regarded as an impurity, which invisibly limits the application range of the master alloy. Therefore, how to effectively reduce the aluminum content in the master alloy produced by the aluminothermic method has become an urgent problem to be solved and the key to further expanding its application field.

[0003] During the aluminothermic reduction process, excess aluminum can indeed significantly increase the recovery rate of the target metal. This is because aluminum, as a reducing agent, can reduce the target metal oxide to a metallic state, while its own oxidation becomes a byproduct. This mechanism ensures a high metal recovery rate, but it also results in 0.5-1.5% aluminum remaining in the alloy. Although this part of residual aluminum improves the metal recovery efficiency, it has become an unavoidable problem in the production of alloy materials that do not require aluminum.

[0004] Therefore, further removing the aluminum element from the master alloy will undoubtedly bring broader prospects for the production and application of the master alloy, and is a topic worthy of study. Summary of the invention

[0005] Purpose of the invention: In view of the deficiencies in the prior art, the present application provides a method for dealumination refining of intermediate alloys by the aluminothermic process.

[0006] Technical solution: The dealumination refining method of the present invention comprises the following steps: placing the intermediate alloy produced by the aluminothermic method in a medium frequency induction furnace, increasing power to increase temperature, adding a dealumination agent after the alloy is completely melted, stirring with a nickel rod for 3-5 minutes after adding to promote the dealumination reaction, the total amount added is calculated according to the aluminum content of the intermediate alloy, and the excess is 30-50%, and after all the dealumination agents are added, refining is performed for 3-10 minutes. During the refining process, the aluminum oxide slag produced by the reaction floats up and combines with calcium fluoride and calcium oxide to form a slag system with a lower melting point. After the refining is completed, the slag is taken out, and the refining is continued for 2-8 minutes, and the alloy is cast into a mold for cooling.

[0007] After cooling, the alloy is crushed to the specified particle size requirement and then sampled for composition testing.

[0008] Specifically, the processing object of the present invention is a master alloy prepared by the aluminothermic method, wherein the aluminum content is about 0.5-1.5% of the total mass of the alloy.

[0009] Specifically, the dealuminizing agent is composed of calcium oxide, calcium fluoride and sodium chlorate in a weight ratio of 1:(4.0-6.0):(6.0-4.0). Calcium oxide and calcium fluoride can reduce the heat density of the reaction between sodium chlorate and aluminum, so that the reaction proceeds smoothly. At the same time, they can combine with the generated aluminum oxide to form a slag system with a lower melting point. This slag system will float on the surface of the alloy in a molten state, which is convenient for removal using a slag removal tool. Preferably, the weight ratio of calcium oxide, calcium fluoride and sodium chlorate is 1:(4.5-5):(4-4.5), and more preferably, the weight ratio of calcium oxide, calcium fluoride and sodium chlorate is 1:5:4. The dealuminizing agent has low cost, easy configuration method, good dealuminizing effect and good versatility.

[0010] Specifically, the amount of dealuminizing agent added is 2.45-7.35% of the mass of the master alloy.

[0011] Further, the amount of the dealuminant added can be 15-50% in excess, that is, the amount of the dealuminant added is 2.8-11% of the mass of the master alloy, preferably, the amount of the dealuminant added is 3.2-9.5% of the mass of the master alloy. Excessive dealuminant ensures complete removal of aluminum, while taking into account that part of the dealuminant may not be completely reacted or consumed.

[0012] Specifically, the dealuminant is added in one addition, two additions (each addition amount is 1:1), or three additions (each addition amount is 1:1:1). Preferably, the dealuminant is added in two additions, each addition amount is 1:1.

[0013] Specifically, the dealuminizer is obtained by the following method: calcium oxide, calcium fluoride, and sodium chlorate are mixed in a mixer according to a weight ratio of 1: (4.0-6.0): (6.0-4.0) and mixed evenly for 30-60 minutes, and then the mixed materials are dried on a drying and frying machine at a temperature above 150° C. for 2 to 4 hours. The purpose is that the dealuminizer is easy to absorb moisture, and drying can remove moisture to avoid generating additional gas during the refining process, which affects the reaction process and product purity. The materials are constantly turned over during the baking process to prevent caking and ensure uniform distribution of the components.

[0014] Beneficial effects: This method can effectively remove residual aluminum in the intermediate alloy produced by the aluminothermic process, stably reducing the aluminum content to less than 0.1%. Refining is also beneficial to the floating of alumina inclusions in the alloy, thereby improving the purity of the alloy. In addition, the process of dealumination does not require the use of high-value raw materials as dealumination agents, and the production cost is low.

[0015] The dealumination refining method of the present invention realizes efficient refining of the master alloy, removes excess aluminum, and simultaneously maintains the purity of other components of the alloy, and is suitable for the production requirements of different types of alloys. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a metallographic photograph of the nickel-niobium alloy before dealumination and refining.

[0017] Figure 2 This is a metallographic photograph of the nickel-niobium alloy obtained after dealumination refining.

[0018] Figure 3 This is a metallographic photograph of the nickel-vanadium alloy before dealumination refining.

[0019] Figure 4 This is a metallographic photograph of the nickel-vanadium alloy after dealumination and refining. DETAILED DESCRIPTION

[0020] The technical solution of the present application is described in detail below through embodiments, but the protection scope of the present application is not limited to the embodiments.

[0021] Example 1

[0022] Preparation of baking dealuminizer: weigh calcium oxide, calcium fluoride and sodium chlorate in a weight ratio of 1:5:4, mix in a mixer for 30 minutes, bake the mixed dealuminizer in a dryer for 3 hours, and turn the material regularly during the baking process to avoid agglomeration. The dealuminizer should be used while hot and removed from the dryer before adding.

[0023] 30kg of nickel-niobium master alloy produced by aluminothermic reduction reaction is loaded into a medium frequency induction furnace. The crucible is a high-purity magnesium oxide crucible. The initial composition of the nickel-niobium alloy is: Ni: 37.56%, Nb: 60.48%, Al: 1.09%, Fe: 0.0480%, Si: 0.067%, C: 0.015%, S: 0.008%, O: 0.087%, N: 0.0253%. Cover the furnace, introduce argon gas, increase the power of 100-120kW to heat until the alloy is completely melted, and add 1.5kg of mixed dealumination agent to the crucible. It can be added twice, assuming 0.75kg each time. After adding, stir with a nickel rod for 1-3 minutes. After the reaction is finished, cover the furnace cover and pass argon to refine for 5 minutes, then open the furnace cover, use a slag scoop to remove the surface slag and put it in a slag basin, add the remaining dealuminant again, and stir for 1-3 minutes. After the reaction is finished, cover the furnace cover and pass argon to refine again for 5 minutes, then open the furnace cover, use a slag scoop to remove the surface slag and put it in a slag basin. Continue to refine for 3 minutes, then cast the alloy into an argon protection mold, cool for 30 minutes, take out the alloy, crush it to an appropriate particle size, and take samples for chemical composition analysis.

[0024] The composition of the nickel-niobium alloy after dealumination refining is: Ni: 38.65%, Nb: 60.22%, Al: 0.062%, Fe: 0.0490%, Si: 0.059%, C: 0.013%, S: 0.006%, O: 0.041%, N: 0.0248%. After dealumination treatment, the aluminum content of the nickel-niobium alloy is reduced from 1.09% to 0.062%, and the dealumination effect is good; and the oxygen content is reduced from 0.087% to 0.041% during the refining process. The metallographic photo of the nickel-niobium alloy after dealumination refining is shown in the figure below. Figure 2 As shown in the metallographic photos, it can be seen that the inclusions after refining have been reduced. This is because the aluminum oxide inclusions in the aluminothermic reduction of nickel and niobium also float up into the slag during the refining process, and the refining also has the effect of deoxidation and slag removal; there is no obvious change in other elements during the refining process. The dealuminizer was added twice, and the dealuminization amount reached 94%.

[0025] Example 2

[0026] Preparation of baking dealuminizer: weigh calcium oxide, calcium fluoride and sodium chlorate in a weight ratio of 1:5:4, mix in a mixer for 30 minutes, bake the mixed dealuminizer in a dryer for 3 hours, and turn the material regularly during the baking process to avoid agglomeration. The dealuminizer should be used while hot and removed from the dryer before adding.

[0027] 30kg of nickel-niobium master alloy produced by aluminum thermal reduction reaction is loaded into a medium frequency induction furnace. The crucible is a high-purity magnesium oxide crucible. The initial composition of the nickel-niobium alloy is: Ni: 37.56%, Nb: 60.48%, Al: 1.09%, Fe: 0.0480%, Si: 0.067%, C: 0.015%, S: 0.008%, O: 0.087%, N: 0.0253%. Cover the furnace cover, pass argon gas, add 100-120kW power to heat until the alloy is completely melted, add 1.5kg of mixed dealuminant to the crucible at one time, stir with a nickel rod for 1-5min, cover the furnace cover after the reaction is completed, pass argon gas for refining for 5min, then open the furnace cover, use a slag spoon to remove the surface slag and put it in a slag basin. Continue refining for 3min, then cast the alloy into an argon-protected mold, cool for 30min, take out the alloy, crush it to an appropriate particle size and take samples for chemical composition analysis.

[0028] The composition of the nickel-niobium alloy after dealumination refining is: Ni: 38.55%, Nb: 60.40%, Al: 0.105%, Fe: 0.0470%, Si: 0.055%, C: 0.014%, S: 0.005%, O: 0.058%, N: 0.0208%. After dealumination treatment, the aluminum content of the nickel-niobium alloy is reduced from 1.09% to 0.103%, and the dealumination effect is slightly worse than that of case 1; the dealumination is added all at once, and the dealumination amount reaches 90.5%.

[0029] Example 3

[0030] Preparation of baking dealuminizer: weigh calcium oxide, calcium fluoride and sodium chlorate in a weight ratio of 1:5:4, mix in a mixer for 30 minutes, bake the mixed dealuminizer in a dryer for 3 hours, and turn the material regularly during the baking process to avoid agglomeration. The dealuminizer should be used while hot and removed from the dryer before adding.

[0031] 30 kg of nickel-niobium master alloy produced by aluminum thermal reduction reaction is loaded into a medium frequency induction furnace. The crucible is a high-purity magnesium oxide crucible. The initial composition of the nickel-niobium alloy is: Ni: 37.56%, Nb: 60.48%, Al: 1.09%, Fe: 0.0480%, Si: 0.067%, C: 0.015%, S: 0.008%, O: 0.087%, N: 0.0253%. Cover the furnace, pass argon, increase the power to 100-120kW and heat until the alloy is completely melted, add 1.5kg of mixed dealumination agent into the crucible three times, 0.5kg each time, stir with a nickel rod for 1-5min, cover the furnace after the reaction is completed, pass argon for refining for 5min, then open the furnace cover, use a slag skimmer to remove the surface slag and put it in a slag basin, repeat this three times, after the third slag skimming, cover the furnace cover, continue refining for 3min, then cast the alloy into an argon protected mold, cool for 30min, take out the alloy, crush it to an appropriate particle size and take samples for chemical composition analysis.

[0032] The composition of the nickel-niobium alloy after dealumination refining is: Ni: 38.64%, Nb: 60.78%, Al: 0.057%, Fe: 0.0478%, Si: 0.065%, C: 0.014%, S: 0.005%, O: 0.068%, N: 0.038%. After dealumination treatment, the aluminum content of the nickel-niobium alloy is reduced from 1.09% to 0.103%, and the dealumination effect is slightly worse than that of Case 1; the dealumination is added all at once, and the dealumination amount reaches 90.5%.

[0033] Addition of dealuminizer Dealumination O N Example 1 Secondary, 1:1 94.7% 0.041% 0.0248% Example 2 Once, 1 94.0% 0.058% 0.0253% Example 3 Three times, 1:1:1 90.5% 0.068% 0.0380%

[0034] From Examples 1 to 3, it can be seen that for nickel-niobium alloy, when the method of the present invention is used for refining and dealumination, the dealumination effect is best when the dealumination agent is added in multiple times. However, as the number of times increases, the overall smelting time will be extended, and the oxidation and nitridation of the melt will be aggravated, thereby increasing the oxygen and nitrogen content. Therefore, when the dealumination agent is added twice, the comprehensive effect is best.

[0035] Example 4

[0036] Preparation of baking dealuminizer: weigh calcium oxide, calcium fluoride and sodium chlorate in a weight ratio of 1:4.5:4.5, mix in a mixer for 40 minutes, bake the mixed dealuminizer in a dryer for 3 hours, and turn the material regularly during the baking process to avoid agglomeration. The dealuminizer should be used while hot and removed from the dryer before adding.

[0037] 20kg of nickel-vanadium master alloy produced by aluminum thermal reduction reaction is loaded into the medium frequency induction furnace. The crucible is a high-purity alumina crucible. The initial composition of the nickel-niobium alloy is: Ni: 40.56%, V: 58.08%, Al: 1.26%, Fe: 0.120%, Si: 0.10%, C: 0.015%, S: 0.003%, O: 0.18%, N: 0.063%. Cover the furnace cover, pass argon gas, add 100-120kW power to heat until the alloy is completely melted, add 1.2kg of mixed dealuminant to the crucible, stir the melt with a nickel rod for 3 minutes to promote the dealuminization reaction, cover the furnace cover after the reaction is completed, pass argon gas for refining for 8 minutes, then open the furnace cover, use a slag spoon to remove the surface slag and put it in the slag basin. Continue refining for 3 minutes, then cast the alloy into an argon-protected mold, cool for 30 minutes, take out the alloy, crush it to an appropriate particle size, and take samples for chemical composition analysis.

[0038] The composition of the nickel-vanadium alloy after dealumination refining is Ni: 41.04%, V: 58.28%, Al: 0.095%, Fe: 0.124%, Si: 0.12%, C: 0.015%, S: 0.003%, O: 0.12%, N: 0.052%. After dealumination treatment, the aluminum content of the nickel-vanadium alloy is reduced from 1.26% to 0.095%, and the dealumination effect is good; and the oxygen content is reduced from 0.18% to 0.12% during the refining process. The metallographic photo of the nickel-vanadium alloy after dealumination refining is shown in the figure below. Figure 4 As shown in the metallographic photograph, it can be seen that the inclusions are reduced after refining. There is no obvious change in other elements during the refining process. The dealuminizer is added all at once, and the dealuminization rate is 89.7%.

[0039] Example 5

[0040] Preparation of baking dealuminizer: weigh calcium oxide, calcium fluoride and sodium chlorate in a weight ratio of 1:4.5:4.5, mix in a mixer for 40 minutes, bake the mixed dealuminizer in a dryer for 3 hours, and turn the material regularly during the baking process to avoid agglomeration. The dealuminizer should be used while hot and removed from the dryer before adding.

[0041] 20 kg of nickel-vanadium master alloy produced by aluminum thermal reduction reaction is loaded into a medium frequency induction furnace. The crucible is a high-purity alumina crucible. The initial composition of the nickel-niobium alloy is: Ni: 40.56%, V: 58.08%, Al: 1.26%, Fe: 0.120%, Si: 0.10%, C: 0.015%, S: 0.003%, O: 0.18%, N: 0.063%. Close the furnace cover, introduce argon, increase the power to 100-120kW and heat until the alloy is completely melted, add 1.2kg of mixed dealumination agent into the crucible twice, 0.6kg each time, stir the melt with a nickel rod for 3 minutes to promote the dealumination reaction, cover the furnace cover after the reaction is completed, introduce argon for refining for 8 minutes, then open the furnace cover, use a slag skimmer to remove the surface slag and put it in a slag basin, repeat this twice, after the second slag skimming, continue refining for 3 minutes, then cast the alloy into an argon-protected mold, cool for 30 minutes, take out the alloy, crush it to an appropriate particle size and take samples for chemical composition analysis.

[0042] The composition of the nickel-vanadium alloy after dealumination refining is Ni: 41.15%, V: 58.08%, Al: 0.085%, Fe: 0.120%, Si: 0.14%, C: 0.010%, S: 0.003%, O: 0.087%, N: 0.072%. After dealumination treatment, the aluminum content of the nickel-vanadium alloy is reduced from 1.26% to 0.085%, and the dealumination effect is good; and the oxygen content is reduced from 0.18% to 0.087% during the refining process, and the nitrogen content increases during the refining process. The dealumination agent is added twice, and the dealumination rate is 93.2%.

[0043] Example 6

[0044] Preparation of baking dealuminizer: weigh calcium oxide, calcium fluoride and sodium chlorate in a weight ratio of 1:4.5:4.5, mix in a mixer for 40 minutes, bake the mixed dealuminizer in a dryer for 3 hours, and turn the material regularly during the baking process to avoid agglomeration. The dealuminizer should be used while hot and removed from the dryer before adding.

[0045] 20 kg of nickel-vanadium master alloy produced by aluminum thermal reduction reaction is loaded into a medium frequency induction furnace. The crucible is a high-purity alumina crucible. The initial composition of the nickel-niobium alloy is: Ni: 40.56%, V: 58.08%, Al: 1.26%, Fe: 0.120%, Si: 0.10%, C: 0.015%, S: 0.003%, O: 0.18%, N: 0.063%. Close the furnace cover, introduce argon, increase the power to 100-120kW and heat until the alloy is completely melted, add 1.2kg of mixed dealumination agent into the crucible in 3 times, 0.4kg each time, stir the melt with a nickel rod for 3 minutes after adding to promote the dealumination reaction, cover the furnace cover after the reaction is completed, introduce argon for refining for 8 minutes, then open the furnace cover, use a slag skimmer to remove the surface slag and place it in a slag basin, repeat the above process 3 times until all the dealumination agent is added, after the third slag skimming, continue refining for 3 minutes, then cast the alloy into an argon-protected mold, cool for 30 minutes, take out the alloy, crush it to an appropriate particle size and take samples for chemical composition analysis.

[0046] The composition of the nickel-vanadium alloy after dealumination refining is Ni: 41.35%, V: 58.18%, Al: 0.070%, Fe: 0.123%, Si: 0.14%, C: 0.013%, S: 0.004%, O: 0.11%, N: 0.112%. After dealumination treatment, the aluminum content of the nickel-vanadium alloy is reduced from 1.26% to 0.070%, and the dealumination effect is good; and the oxygen content is reduced from 0.18% to 0.11% during the refining process, but it increases due to the addition of two times, and the nitrogen content increases from 0.063% to 0.112%. The dealumination agent is added twice, and the dealumination rate is 94.4%.

[0047] Addition of dealuminizer Dealumination O N Example 4 once 89.7% 0.12% 0.052% Example 5 Secondary, 1:1 93.2% 0.087% 0.072% Example 6 Three times, 1:1:1 94.4% 0.11% 0.112%

[0048] From Examples 4 to 6, it can be seen that for nickel-vanadium alloy, when the method of the present invention is used to refine and dealuminate, the dealuminizer is added twice, and the comprehensive effect is the best. The dealuminizer is added three times, and although the dealuminizer effect is improved, the degree of improvement is limited. Vanadium and nitrogen react easily, and adding the dealuminizer three times increases the smelting time, causing a certain degree of oxidation and nitridation, resulting in an increase in the oxygen and nitrogen content compared to adding it twice.

[0049] The above description is only a preferred embodiment of the present application and is not intended to limit the present application.

Claims

1. A method for dealumination refining of master alloy by aluminothermic process, characterized in that: Place the intermediate alloy produced by the aluminothermic method in a medium frequency induction furnace, increase the power to increase the temperature, add the dealuminizer after the alloy is completely melted, stir with a nickel rod for 3-5 minutes after adding to promote the dealuminization reaction, and after all the dealuminizers are added, refine for 3-10 minutes. During the refining process, the alumina slag produced by the reaction floats up and combines with calcium fluoride and calcium oxide to form a slag system with a lower melting point. After the refining is completed, take out the slag, continue refining for 2-8 minutes, and cast the alloy into a mold to cool.

2. The method for dealumination refining of master alloy by the aluminothermic process according to claim 1, characterized in that: The aluminothermic master alloy is a master alloy prepared by the aluminothermic method, wherein the content of aluminum impurities is 0.5-1.5% of the total mass of the alloy.

3. The method for dealumination refining of master alloy by the aluminothermic process according to claim 1, characterized in that: The dealuminizing agent is composed of calcium oxide, calcium fluoride and sodium chlorate in a weight ratio of 1:(4.0-6.0):(6.0-4.0).

4. The method for dealumination refining of master alloy by the aluminothermic process according to claim 1, characterized in that: The dealuminizing agent is composed of calcium oxide, calcium fluoride and sodium chlorate in a weight ratio of 1:(4.5-5):(4-4.5).

5. The method for dealumination refining of master alloy by the aluminothermic process according to claim 1, characterized in that: The dealuminizing agent is composed of calcium oxide, calcium fluoride and sodium chlorate in a weight ratio of 1:5:

4.

6. The method for dealumination refining of master alloy by the aluminothermic process according to claim 1, characterized in that: The amount of dealuminizer added is 2.45-7.35% of the mass of the master alloy.

7. The method for dealumination refining of master alloy by the aluminothermic process according to claim 1, characterized in that: The amount of dealuminizing agent added is 3.2-9.5% of the mass of the master alloy.

8. The method for dealumination refining of master alloy by the aluminothermic process according to claim 1, characterized in that: The dealuminant is added in the following manners: once; twice, with the amount added each time being 1:1; or three times, with the amount added each time being 1:1:

1.

9. The method for dealumination refining of master alloy by the aluminothermic process according to claim 1, characterized in that: The dealuminizing agent is added in two times, with the amount added each time being 1:

1.

10. The method for dealumination refining of master alloy by the aluminothermic process according to claim 1, characterized in that: The dealuminizing agent is obtained by the following method: calcium oxide, calcium fluoride and sodium chlorate are mixed in a mixer in a weight ratio of 1: (4.0-6.0): (6.0-4.0) and mixed evenly for 30-60 minutes, and then the mixed materials are dried on a drying and frying machine at a temperature above 150° C. for 2 to 4 hours, and the materials are constantly turned during the baking process to avoid caking.