Brass strip and preparation method and application thereof

Through batch smelting, inflating and demulsification and heat treatment processes, the surface cracking problem of H65 brass and steel strips are solved, and low-strength and high elongation brass strips are prepared to meet the rolling needs of copper-steel composite strips and reduce the Production costs and expand military applications.

CN118932199APending Publication Date: 2024-11-12JINTIAN COPPER GROUP CORP NINGBO
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410999348.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the production cost of using H90 or H95 brass to make bullet shells is relatively high, and the surface cracking occurs when the H65 brass is rolled and composited with steel strips, making it impossible to effectively realize rolling and composited.

Method used

By using batching smelting + inflatable demulsification, hot rolling + online heat treatment, multiple heat treatment and rolling processes, the impurity content is controlled by blowing compressed air, reducing the strength of the alloy and improving the elongation, ensuring the copper-steel composite belt Rolling composite performance.

Benefits of technology

Brass strips with extremely low strength, excellent elongation and good plasticity were prepared to meet the rolling and composite performance requirements of copper-steel composite strips, reduce production costs, and have broad application prospects in the military industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a brass strip and a preparation method and application thereof. The preparation method comprises the steps of ingredient smelting, air inflation impurity removal, semi-continuous casting red ingot casting, hot rolling, online heat treatment, rough rolling, first heat treatment, first intermediate rolling, second heat treatment, second intermediate rolling, third heat treatment, finished product rolling and finished product heat treatment. The brass strip with extremely low strength, excellent elongation and good plasticity is prepared through matching of processes of ingredient smelting, aeration impurity removal, hot rolling, online heat treatment, multiple heat treatment and rolling processing rate control, and the requirement of the rolling composite performance of the copper-steel composite strip is met. The hardness of the brass strip product is smaller than 56HV, the tensile strength is smaller than 260MPa, the ductility is larger than 55%, the grain size of the finished product is 60-90 microns, the brass strip product can replace H90 and H95 brass to be used for preparing a copper-steel composite strip for a bullet shell, the production cost is greatly reduced, and the brass strip has wide application prospects in the military industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copper alloys, and in particular to a brass strip and a preparation method and application thereof. Background Art

[0002] Bullets are composed of four parts: shell, primer, propellant and warhead. Among the traditional shell materials, copper is the most ideal shell material, with advantages such as good ductility, less wear on firearms and not easy to jam. At present, most military industries use H90 or H95 brass to manufacture bullet shells. Brass has excellent deep drawing performance and corrosion resistance. At the same time, brass has lubrication, which can reduce the wear on the barrel, chamber and rifling during shooting and increase the service life of firearms. Some military enterprises use copper-steel composite belts to replace original brass belts to produce bullet shells. Copper-steel composite belts have the common characteristics of high strength, good heat resistance, cold processing, corrosion resistance and wear resistance of composite materials, while retaining the lubrication properties of brass surface.

[0003] The patent document with publication number CN111411257A discloses a production process of high-plastic brass strip for producing H90 bullet shells, including the following steps: P1, batching; P2, melting and casting; P3, hot rolling; P4, milling; P5, rough rolling; P6, primary annealing; P7, intermediate rolling; P8, secondary annealing; P9, finishing rolling; P10, surface treatment; P11, shearing; P12, inspection and packaging. The invention can ensure crystallization refinement and improve the internal material properties by treating the molten raw materials in the melting and pouring stage, and improve the surface quality of the plate through multiple surface and edge treatments during the rolling process. At the same time, the protective gas is filled during annealing, combined with passivation packaging, storage oxidation can be avoided, and the product quality of the brass strip can be improved.

[0004] The patent document with publication number CN112620347A discloses a processing technology for producing high-plastic brass strips for H90 bullet shells, which includes the following steps: A. Raw material batching, cleaning and drying; B. Melting and casting; C. Hot rolling and milling; D. Rough rolling and primary annealing; E. Intermediate rolling and secondary annealing; F. Finishing rolling; G. Surface treatment and shearing; H. Surface anti-corrosion coating; I. Inspection and packaging. The invention cleans the raw materials and simultaneously coats the surface of the high-plastic brass strip with anti-corrosion coating, thereby achieving the advantages of cleaning the raw material surface to remove impurities and coating the surface of the high-plastic brass strip with anti-corrosion coating for long-term storage, thereby improving the subsequent processing quality of the high-plastic brass strip.

[0005] However, H90 or H95 brass is mostly used to manufacture bullet casings in the prior art, and the production cost is relatively high. Now military enterprises have proposed to use H65 instead of H90 or H95 to produce copper-steel composite strips to manufacture bullet casings to further reduce costs. However, the hardness and tensile strength of H65 produced by current production technology are relatively high. When it is rolled and compounded with steel strips, the brass layer on the surface of the composite strip cracks, and the rolling compounding of H65 and steel strip cannot be effectively achieved. Therefore, based on industry application requirements, it is urgent to develop an H65 brass strip for copper-steel composite strips with extremely low strength, excellent elongation and good plasticity to meet the rolling compounding performance requirements of copper-steel composite strips. Summary of the invention

[0006] In order to solve the above problems, the present invention provides a method for preparing a brass strip. The method uses H65 brass as raw material, and prepares the brass strip through processes such as batching smelting + inflation and impurity removal, hot rolling + online heat treatment, which greatly reduces the production cost. The brass strip produced by the method has extremely low strength, excellent elongation and good plasticity.

[0007] A method for preparing a brass strip comprises the following steps:

[0008] Ingredient smelting + gasification and impurity removal → semi-continuous casting red ingot casting → hot rolling + online heat treatment → rough rolling → first heat treatment → first intermediate rolling → second heat treatment → second intermediate rolling → third heat treatment → finished product rolling → finished product heat treatment;

[0009] Among them, in the batch smelting + charging and de-impurity process, the raw material ratio satisfies Cu: 63.5-66wt%, and the balance is Zn and unavoidable impurities; the conditions for charging and de-impurity are: blowing compressed air into the smelting furnace, the blowing flow rate is 10-20L / min, the pressure is 0.02-0.1MPa, and the blowing time is 20-40min.

[0010] The present invention adopts an aeration impurity removal process, in which compressed air is blown in, and oxygen atoms in the compressed air fully react with impurity elements in the copper liquid to generate metal oxide slag, which is then fished out, thereby reducing the content of impurity elements in the copper liquid and obtaining a copper alloy with excellent plasticity and lower strength.

[0011] Preferably, in the batch smelting + aeration and impurity removal process, compressed air is blown into the bottom of the smelting furnace, the blowing flow rate is 10-20 L / min, the pressure is 0.02-0.1 MPa, the blowing time is 20-40 min, and the oxidized slag is removed after the molten copper is still for 10-15 min.

[0012] In the batch smelting + aeration and impurity removal process, electrolytic copper is added to a smelting furnace to heat and melt, and then the temperature is raised to 1100-1140° C. A bottom blowing generator is used to blow compressed air, with a blowing flow rate of 10-20 L / min, a pressure of 0.02-0.1 MPa, and a blowing time of 20-40 min. After the copper liquid is still for 10-15 min, the oxidized slag is removed. Since electrolytic copper contains a certain amount of impurity elements such as Fe, P, Ni, Al and Sn, which have the effect of refining grain structure or strengthening alloy properties through solid solution, the air can be blown into the bottom-blown generator of the smelting furnace to allow the oxygen in the air to be fully dispersed in the copper liquid. Then the oxygen atoms react with the impurity elements such as Fe, P, Ni, Al and Sn in the copper liquid to generate metal oxide slag. At the same time, the blown-in air contains a large amount of nitrogen. The nitrogen is blown into the bottom of the melt through the bottom-blown generator, and then forms dispersed small bubbles that float from the bottom of the melt to the surface of the copper liquid and are discharged. In the process of nitrogen floating and discharging, the nitrogen will adsorb the oxide slag generated in the melt and bring it to the surface of the melt, so that the nitrogen also plays a role in refining and removing slag, purifying the copper water. After the impurity removal by inflation, the content of impurity elements is controlled at P < 0.0005wt%, Si < 0.001wt%, Al < 0.0005wt%, Sn < 0.001wt%, Mg < 0.0005wt%, Fe < 0.001wt%, Ni < 0.001wt%. With the reduction of impurity elements, the performance of the cast alloy is better in plasticity and lower in strength under the same process, which is conducive to the composite with the steel strip. Preferably, the blowing flow rate is 10-20L / min, the pressure is 0.02-0.06MPa, and the blowing time is 20-40min.

[0013] Preferably, in the hot rolling + online heat treatment process, the ingot heating temperature is 840-880°C, the holding time is 2-3h, the hot rolling start temperature is 820-850°C, the hot rolling final rolling temperature is above 550°C, after the hot rolling final rolling material temperature drops to 550°C, the hot-rolled strip is coiled online and placed in a heat treatment furnace within 10 minutes, and the temperature of the heat treatment furnace is adjusted to 580-610°C. After holding for 2-3 hours, it is cooled to below 80°C by air cooling.

[0014] The molten metal after impurities removal is semi-continuously cast into red ingots, and the obtained ingots are subjected to hot rolling + online heat treatment. In the hot rolling + online heat treatment process, the ingot heating temperature is 840-880°C, the holding time is 2-3h, the hot rolling start temperature is 820°C-850°C, and the hot rolling final rolling temperature is ensured to be above 550°C. After the hot rolling final rolling material temperature drops to 550°C, the hot-rolled strip is rolled online and placed in a heat treatment furnace within 10 minutes, and the heat treatment furnace temperature is adjusted to 580-610°C, kept warm for 2-3 hours, and then cooled to below 80°C by air cooling, and the average grain size is controlled to 120-180μm. The present invention controls the average grain size of the alloy to 120-180μm through the hot rolling + online heat treatment process, ensuring that the target performance product is obtained after the alloy is subsequently rolled and heat treated.

[0015] Preferably, in the semi-continuous casting of red ingots, the crystallizer adopts primary cooling without secondary cooling, and the primary cooling water flow rate is 30-50m 3 / h, water pressure is 0.4~0.6MPa, water inlet temperature is 20~28℃, water outlet temperature is controlled at 40~50℃, ingot temperature out of crystallizer is 600~700℃, and then air-cooled to below 80℃. Red ingot casting is adopted, there is only one cooling water during the casting process, and the ingot temperature out of crystallizer reaches above 600℃. This casting method has low cooling intensity, and the ingot structure of the cast is coarse equiaxed crystal. Since the grain structure is hereditary, the grain structure is larger after the finished product, the grain structure is large, the strength of the material is low, which is conducive to the composite with the steel strip.

[0016] Preferably, in the rough rolling process, the rough rolling processing rate is controlled at 40-60%. When the rough rolling processing rate is less than 40%, the cold processing fiber texture of the copper strip is not obvious due to insufficient processing deformation. If high temperature annealing is performed, the annealing recrystallization grain structure will be uneven, that is, there will be abnormally coarse and fine grains, and the cold processing plasticity of the alloy strip will be reduced, resulting in local cracking when the copper strip is compounded in the later stage. However, if the processing rate exceeds 60%, due to the excessive processing rate, the fiber texture is obvious after cold processing, the grains of the organization are severely broken, and the grains are difficult to grow significantly during the subsequent high-temperature annealing, which will lead to the failure to meet the grain size requirements of this alloy control. Due to the small grain size, (according to the Hall-Petch formula σs=σ0+Kd~1 / 2 (σs is the yield strength; σ0 is the yield strength of the single crystal, which is a constant; K is the influence coefficient of the grain boundary on the strength, which is a constant; d is the average diameter of the grain), it can be seen that the finer the grain within the grain size range, the higher the strength of the material) the brass layer on the surface of the composite strip cracks, and the rolling composite of H65 and steel strip cannot be effectively achieved.

[0017] By controlling the rough rolling process processing rate at 40-60%, combined with the first heat treatment process, bell-type furnace annealing is adopted, and the protective atmosphere is a reducing atmosphere of 70-80% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 550-600℃ at a heating rate of 100-150℃ / h and keep it at that temperature for 4-6h, and then cool it to room temperature by air cooling at a rate of 60-90℃ / h. After the first high-temperature heat treatment, the average grain size of the material is controlled at 100-150μm, which provides a suitable grain size for subsequent processing, and facilitates the performance of the finished product to be controlled within the hardness of <56HV, tensile strength of <260MPa, and elongation of >55%.

[0018] Similarly, the processing rates of the first intermediate rolling and the second intermediate rolling are preferably controlled at 40-60%, and the processing rate of the finished product rolling is preferably controlled at 45-55%, so as to avoid abnormally uneven grains after high-temperature annealing due to too small a processing rate, and to avoid fine grains after annealing due to too large a processing rate.

[0019] Similarly, in the second and third heat treatment processes, bell-type furnace annealing is used to heat the alloy copper strip to 540-580°C and 520-560°C at a heating rate of 100-150°C / h, respectively, and keep warm for 4-6 hours, and then cool it to room temperature at a rate of 60-90°C / h by air cooling. The protective atmosphere is a reducing atmosphere with 70-80% H 2 + the balance of nitrogen gas. The average grain size of the material is controlled within 80-120 μm by the second heat treatment, and the average grain size of the material is controlled within 75-110 μm by the third heat treatment.

[0020] The three heat treatments of the present invention are coupled, and the previous heat treatment has a direct impact on the subsequent heat treatment, and ultimately has a direct impact on the grain size and performance of the finished product. Because as the cold working proceeds, the thickness of the previous heat treatment is thinner than the thickness of the product of the thicker heat treatment, so the temperature of each heat treatment will be slightly reduced, thereby avoiding the abnormal growth of grain size due to excessive heat treatment temperature. At the same time, in order to ensure that during the heating and cooling process of the heat treatment process, its temperature partially exceeds the recrystallization temperature of the alloy, and avoid the unevenness of the treated grain size due to the large span of the heating and cooling period during the heat treatment process, the heat treatment is heated at a rate of 100 to 150°C / h, and then cooled by air cooling at a rate of 60 to 90°C / h.

[0021] Preferably, in the finished product heat treatment process, bell-type furnace annealing is adopted, and the protective atmosphere is a reducing atmosphere with 70-80% H 2+ Residual nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 450-480℃ at a heating rate of 100-150℃ / h and keep it warm for 4-6h, and then cool it to room temperature by air cooling at a rate of 60-90℃ / h, and control the average grain size to 60-90μm. The heat treatment temperature of the finished product is controlled at 450-480℃ and kept warm for 4-6h. If the heat treatment heating temperature is lower than 450℃ or the holding time is lower than 4h, the strength of the finished material after heat treatment will be higher than the design requirements of the product, and the small grain size will further increase the strength of the material. However, if the heat treatment heating temperature is higher than 480℃ or the holding time is higher than 6h, the grain size of the finished product is greater than 90μm. Due to the excessive grain size of the finished product, the surface of the copper strip will show orange peel phenomenon, pits will appear when compounded with the steel strip, and even local cracks will appear, which will not meet the product requirements for compounding with the steel strip.

[0022] Preferably, the strip is cleaned after the first heat treatment, the second heat treatment, the third heat treatment and the final heat treatment.

[0023] Preferably, in the cleaning process, the intermediate tension of the unwinding and pickling S roller group and the winding tension are controlled at 10N / mm 2 Because this alloy product is required to be a special soft product, if the tension is too large, it will cause the alloy strip to produce longitudinal tensile deformation, and the material strength will increase. Therefore, in order to avoid this alloy strip when cleaning, the middle tension of the unwinding and pickling S roller group and the winding tension are required to be controlled at 10N / mm 2 To avoid the increase of strength after plastic micro-deformation of the strip.

[0024] The present invention also provides a brass strip prepared by the preparation method, which has extremely low strength, excellent elongation and good plasticity.

[0025] Preferably, the brass strip has a hardness of less than 56 HV, a tensile strength of less than 260 MPa, and an elongation of more than 55%.

[0026] Preferably, the average grain size of the brass strip is 60-90 μm.

[0027] The present invention also provides the use of the brass strip in preparing a copper-steel composite strip for bullet casings. The brass strip of the present invention has extremely low strength and excellent elongation, and good plasticity, meets the rolling composite performance requirements of the copper-steel composite strip, and can be used to prepare the copper-steel composite strip for producing bullets.

[0028] Compared with the prior art, the present invention has at least the following beneficial effects:

[0029] The present invention prepares a brass strip with extremely low strength, excellent elongation and good plasticity by combining batch melting + gas impurity removal, hot rolling + online heat treatment, multiple heat treatments and rolling processes. The brass strip meets the rolling composite performance requirements of the copper-steel composite strip, has a hardness of less than 56HV, a tensile strength of less than 260MPa, an elongation of more than 55%, and a finished product grain size of 60 to 90μm. The brass strip can replace H90 and H95 for producing copper-steel composite strips for manufacturing bullet casings, greatly reducing production costs, and has broad application prospects in the military industry. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments.

[0031] The chemical composition of the copper alloy strip in the embodiment of the present invention is shown in Table 1.

[0032] Table 1 Chemical composition of copper alloy strip (wt%)

[0033] Cu Zn and inevitable impurities 63.5~66 margin

[0034] The preparation process of the copper alloy strip in the embodiment of the present invention is: batch smelting + aeration and impurity removal → semi-continuous casting red ingot casting → hot rolling + online heat treatment → milling → rough rolling → trimming → first high-temperature heat treatment → cleaning → first intermediate rolling → second high-temperature heat treatment → cleaning → second intermediate rolling → third high-temperature heat treatment → cleaning → finished product rolling → finished product heat treatment → cleaning → finished product stripping and packaging. The specific steps are as follows:

[0035] S1. Ingredient smelting + aeration and impurity removal

[0036] Add electrolytic copper to the smelting furnace to heat and melt, then raise the temperature to 1100-1140℃, use the bottom blowing generator of the smelting furnace to blow in compressed air, the blowing flow rate is 10-20L / min, the pressure is 0.02-0.06MPa, the blowing time is 20-40min, wait for the copper liquid to stand for 10-15min, and then remove the oxide slag. After oxygenation and impurity removal, the impurity elements are controlled to P < 0.0005wt%, Si < 0.001wt%, Al < 0.0005wt%, Sn < 0.001wt%, Mg < 0.0005wt%, Fe < 0.001wt%, Ni < 0.001wt%. Then add zinc ingots according to the composition ratio, keep warm for 20-30 minutes, then remove the slag, and start casting.

[0037] S2, Semi-continuous casting red ingot casting

[0038] The temperature of the copper liquid is controlled at 1100-1120℃, the frequency of the vibrator is 30-50 times / min, the amplitude is 3-6mm, the crystallizer is covered with anhydrous borax during the entire casting process, and the casting speed of the ingot is 50-80mm / min. The crystallizer adopts primary cooling without secondary cooling, and the primary cooling water flow is 30-50m 3 / h, water pressure 0.4~0.6MPa, water inlet temperature 20~28℃, water outlet temperature controlled at 40~50℃, ingot temperature out of crystallizer at 600~700℃, then air-cooled to below 80℃ for 36 hours, ingot drawing specification is 230*620mm*8000mm.

[0039] S3, hot rolling + online heat treatment

[0040] The ingot heating temperature is 840-880℃, the holding time is 2-3h, the hot rolling starting temperature is 820℃-850℃, hot rolling to 12mm thickness, and at the same time, the hot rolling final rolling temperature is ensured to be above 550℃, and the width of the hot rolling widened strip is 650±5mm. After the hot rolling final rolling material temperature drops to 550℃, the hot-rolled strip is coiled online and placed in the heat treatment furnace within 10 minutes, and the heat treatment furnace temperature is adjusted to 580-610℃, kept warm for 2-3 hours, and then air-cooled to below 80℃, and the average grain size is controlled to 120-180μm.

[0041] S4, milling surface

[0042] The single-sided milling amount is 0.5~1.5mm.

[0043] S5, Rough Rolling

[0044] The rough rolling processing rate is controlled at 40-60%.

[0045] S6, trimming

[0046] The single-side shearing is 7-10mm, and the belt width after shearing is 630±0.5mm.

[0047] S7, first high temperature heat treatment

[0048] The bell-type furnace is used for annealing, and the protective atmosphere is a reducing atmosphere of 70-80% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 550-600℃ at a heating rate of 100-150℃ / h and keep it at that temperature for 4-6h, and then cool it to room temperature by air cooling at a rate of 60-90℃ / h. The average grain size is controlled at 100-150μm.

[0049] S8. Cleaning

[0050] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 7-9, and the solution temperature is 60-70°C; then pickling is performed, the sulfuric acid concentration is 100-130g / l, the temperature is ≤40°C, and the Cu in the acid solution 2+ ≤1.2g / l; clean and dry, the oven temperature is 65-70℃.

[0051] S9, first intermediate rolling

[0052] The intermediate rolling processing rate is controlled at 40-60%.

[0053] S10, Second high temperature heat treatment

[0054] The bell-type furnace is used for annealing, and the protective atmosphere is a reducing atmosphere of 70-80% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 540-580℃ at a heating rate of 100-150℃ / h and keep it at that temperature for 4-6h, and then cool it to room temperature by air cooling at a rate of 60-90℃ / h. The average grain size is controlled at 80-120μm.

[0055] S11. Cleaning

[0056] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 7-9, and the solution temperature is 60-70°C; then pickling is performed, the sulfuric acid concentration is 100-130g / l, the temperature is ≤40°C, and the Cu in the acid solution 2+ ≤1.2g / l; clean and dry, the oven temperature is 65-70℃.

[0057] S12, second intermediate rolling

[0058] The intermediate rolling processing rate is controlled at 40-60%.

[0059] S13, the third high temperature heat treatment

[0060] The bell-type furnace is used for annealing, and the protective atmosphere is a reducing atmosphere of 70-80% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 520-560℃ at a heating rate of 100-150℃ / h and keep it at that temperature for 4-6h, and then cool it to room temperature by air cooling at a rate of 60-90℃ / h. The average grain size is controlled at 75-110μm.

[0061] S14. Cleaning

[0062] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 7-9, and the solution temperature is 60-70°C; then pickling is performed, the sulfuric acid concentration is 100-130g / l, the temperature is ≤40°C, and the Cu in the acid solution 2+≤1.2g / l; clean and dry, the oven temperature is 65-70℃.

[0063] S15, finished product rolling

[0064] The finished product rolling processing rate is controlled at 45-55%.

[0065] S16, Finished product heat treatment

[0066] The bell-type furnace is used for annealing, and the protective atmosphere is a reducing atmosphere of 70-80% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 450-480℃ at a heating rate of 100-150℃ / h and keep it at that temperature for 4-6h, and then cool it to room temperature by air cooling at a rate of 60-90℃ / h. The average grain size of the finished product is controlled at 60-90μm.

[0067] S17, cleaning

[0068] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 7-9, and the solution temperature is 60-70°C; then pickling is performed, the sulfuric acid concentration is 100-130g / l, the temperature is ≤40°C, and the Cu in the acid solution 2+ ≤1.2g / l; cleaning and drying, the oven temperature is 65-70℃, during the cleaning process, the tension between the unwinding and pickling S roller group and the winding tension are controlled at 10N / mm 2 Within.

[0069] S18, finished product stripping and packaging.

[0070] The copper alloy strip prepared in the embodiment of the present invention has a thickness of 0.5-1.0 mm, a product hardness of less than 56 HV, a tensile strength of less than 260 MPa, an elongation of more than 55%, and a finished grain size of 60-90 μm. It has extremely low strength and excellent elongation, good plasticity, and can meet the rolling composite performance requirements of the copper-steel composite strip.

[0071] The technical solutions and effects of the present invention are illustrated below with reference to specific embodiments.

[0072] The specific compositions of the copper alloy strips of Examples 1 to 4 and Comparative Examples 1 to 3 are shown in Table 2, and the key process parameters are shown in Table 3.

[0073] Example 1

[0074] The preparation steps of the copper alloy strip of this embodiment are as follows:

[0075] 1) Ingredient smelting + aeration and impurity removal

[0076] Add electrolytic copper to the smelting furnace to heat and melt, then raise the temperature to 1135℃, use the bottom blowing generator of the smelting furnace to blow in compressed air, the blowing flow rate is 18L / min, the pressure is 0.055MPa, the blowing time is 34min, wait for the copper liquid to stand for 12min, and then remove the oxide slag. After oxygenation and impurity removal, the impurity elements are controlled at P<0.0005wt%%,Si<0.001wt%%,Al<0.0005wt%%,Sn<0.001wt%%,Mg<0.0005wt%%%,Fe<0.001wt%%%,Ni<0.001wt%%. Then add zinc ingots according to the composition ratio, keep warm for 20-30 minutes, then remove the slag, and start casting.

[0077] 2) Semi-continuous casting of red ingots

[0078] The temperature of the copper liquid is controlled at 1118℃, the frequency of the vibrator is 46 times / min, the amplitude is 4.5mm, the crystallizer is covered with anhydrous borax during the entire casting process, and the casting speed of the ingot is 72mm / min. The crystallizer adopts primary cooling without secondary cooling, and the primary cooling water flow is 41m 3 / h, water pressure 0.51MPa, water inlet temperature 25℃, water outlet temperature controlled at 42℃, ingot temperature out of crystallizer at 680℃, then air-cooled to below 80℃ for 36 hours, ingot drawing specification is 230*620mm*8000mm.

[0079] 3) Hot rolling + online heat treatment

[0080] The ingot heating temperature is 860℃, the holding time is 2.5h, the hot rolling starting temperature is 835℃, hot rolling is to 12mm thick, and the hot rolling final rolling temperature is 575℃, and the width of the hot rolling widening is 650±5mm. After the hot rolling final rolling material temperature drops to 550℃, the hot rolled strip is coiled online and placed in the heat treatment furnace within 10 minutes, and the heat treatment furnace temperature is adjusted to 600℃, kept warm for 2.4 hours, and then air cooled to below 80℃, and the average grain size is controlled at 148μm.

[0081] 4) Milling

[0082] The single-sided milling amount is 0.75mm, and the milling surface is 10.5mm thick.

[0083] 5) Rough rolling

[0084] Rough rolling to 6mm, processing rate 42.86%.

[0085] 6) Trimming

[0086] The single-side shearing is 7-10mm, and the belt width after shearing is 630±0.5mm.

[0087] 7) First high temperature heat treatment

[0088] The bell-type furnace annealing was adopted, and the protective atmosphere was a reducing atmosphere of 74% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 590℃ at a heating rate of 128℃ / h and keep it at that temperature for 5h, and then cool it to room temperature at a rate of 82℃ / h. The average grain size is controlled at 136μm.

[0089] 8) Cleaning

[0090] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 8.1, and the solution temperature is 67°C; then pickling is performed, the sulfuric acid concentration is 125g / l, the temperature is 37°C, and the Cu in the acid solution is 2+ ≤1.2g / l; clean and dry, the oven temperature is 68℃.

[0091] 9) First intermediate rolling

[0092] Medium rolling to 3mm, processing rate 50%.

[0093] 10) Second high temperature heat treatment

[0094] The bell-type furnace annealing was adopted, and the protective atmosphere was a reducing atmosphere of 76% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 575℃ at a heating rate of 142℃ / h and keep it at that temperature for 4.8h, and then cool it to room temperature at a rate of 79℃ / h. The average grain size is controlled at 110μm.

[0095] 11) Cleaning

[0096] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 7.9, and the solution temperature is 67°C; then pickling is performed, the sulfuric acid concentration is 118g / l, the temperature is 35°C, and the Cu in the acid solution is 2+ ≤1.2g / l; clean and dry, the oven temperature is 69℃.

[0097] 12) Second intermediate rolling

[0098] The milling process was continued until 1.4 mm and the processing rate was controlled at 53.33%.

[0099] 13) The third high temperature heat treatment

[0100] The bell-type furnace annealing was adopted, and the protective atmosphere was a reducing atmosphere of 74% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 545℃ at a heating rate of 126℃ / h and keep it at that temperature for 5h, and then cool it to room temperature at a rate of 72℃ / h. The average grain size is controlled at 98μm.

[0101] 14) Cleaning

[0102] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 8.3, and the solution temperature is 64°C; then pickling is performed, the sulfuric acid concentration is 119g / l, the temperature is 32°C, and the Cu in the acid solution is 2+ ≤1.2g / l; clean and dry, the oven temperature is 66℃.

[0103] 15) Finished product rolling

[0104] The finished product is rolled to 0.7mm and the processing rate is controlled at 50%.

[0105] 16) Finished product heat treatment

[0106] The bell-type furnace annealing was adopted, and the protective atmosphere was a reducing atmosphere of 77% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 470℃ at a heating rate of 132℃ / h and keep it at that temperature for 5.2h, and then cool it to room temperature at a rate of 85℃ / h. The average grain size of the finished product is controlled at 85μm.

[0107] 17) Cleaning

[0108] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 8.1, and the solution temperature is 67°C; then pickling is performed, the sulfuric acid concentration is 121g / l, the temperature is 34°C, and the Cu in the acid solution is 2+ ≤1.2g / l; cleaning and drying, the oven temperature is 68℃, during the cleaning process, the tension between the unwinding and pickling S roller group and the winding tension are controlled at 7.5N / mm 2 .

[0109] 18) Finished products are striped and packaged.

[0110] Example 2

[0111] The preparation steps of the copper alloy strip of this embodiment are as follows:

[0112] 1) Ingredient smelting + aeration and impurity removal

[0113] Add electrolytic copper to the smelting furnace to heat and melt, then raise the temperature to 1125℃, use the bottom blowing generator of the smelting furnace to blow in compressed air, the blowing flow rate is 17L / min, the pressure is 0.045MPa, the blowing time is 35min, wait for the copper liquid to be still for 13min, and then remove the oxide slag. After oxygenation and impurity removal, the impurity elements are controlled at P<0.0005wt%%,Si<0.001wt%%,Al<0.0005wt%%,Sn<0.001wt%%,Mg<0.0005wt%%%,Fe<0.001wt%%%,Ni<0.001wt%%. Then add zinc ingots according to the composition ratio, keep warm for 20-30 minutes, then remove the slag, and start casting.

[0114] 2) Semi-continuous casting of red ingots

[0115] The temperature of the copper liquid is controlled at 1115℃, the frequency of the vibrator is 45 times / min, the amplitude is 5mm, the crystallizer is covered with anhydrous borax during the entire casting process, and the casting speed of the ingot is 68mm / min. The crystallizer adopts primary cooling without secondary cooling, and the primary cooling water flow is 41m 3 / h, water pressure 0.52MPa, water inlet temperature 25℃, water outlet temperature controlled at 47℃, ingot temperature out of crystallizer at 680℃, then air-cooled to below 80℃ for 36 hours, ingot drawing specification is 230*620mm*8000mm.

[0116] 3) Hot rolling + online heat treatment

[0117] The ingot heating temperature is 865℃, the holding time is 2.6h, the hot rolling starting temperature is 841℃, hot rolling is carried out to a thickness of 12mm, and the hot rolling final rolling temperature is ensured to be 585℃, and the width of the hot rolling widened strip is 650±5mm. After the hot rolling final rolling material temperature drops to 550℃, the hot-rolled strip is coiled online and placed in the heat treatment furnace within 10 minutes, and the heat treatment furnace temperature is adjusted to 595℃, kept warm for 2.6 hours, and then air-cooled to below 80℃, and the average grain size is controlled at 161μm.

[0118] 4) Milling

[0119] The single-sided milling amount is 0.75mm, and the milling surface is 10.5mm thick.

[0120] 5) Rough rolling

[0121] Rough rolling to 5.5mm, the processing rate is controlled at 47.62%.

[0122] 6) Trimming

[0123] The single-side shearing is 7-10mm, and the belt width after shearing is 630±0.5mm.

[0124] 7) First high temperature heat treatment

[0125] The bell-type furnace annealing was adopted, and the protective atmosphere was a reducing atmosphere of 73% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 590℃ at a heating rate of 128℃ / h and keep it at that temperature for 4.6h, and then cool it to room temperature at a rate of 75℃ / h. The average grain size is controlled at 138μm.

[0126] 8) Cleaning

[0127] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 8, and the solution temperature is 64°C; then pickling is performed, the sulfuric acid concentration is 121g / l, the temperature is 34°C, and the Cu in the acid solution is 2+ ≤1.2g / l; clean and dry, the oven temperature is 68℃.

[0128] 9) First intermediate rolling

[0129] Medium rolling to 2.8mm, processing rate 49.09%.

[0130] 10) Second high temperature heat treatment

[0131] The bell-type furnace annealing was adopted, and the protective atmosphere was a reducing atmosphere of 76% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 565℃ at a heating rate of 132℃ / h and keep it at that temperature for 4.9h, and then cool it to room temperature at a rate of 82℃ / h. The average grain size is controlled at 105μm.

[0132] 11) Cleaning

[0133] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 7.8, and the solution temperature is 68°C; then pickling is performed, the sulfuric acid concentration is 119g / l, the temperature is 32°C, and the Cu in the acid solution is 2+ ≤1.2g / l; clean and dry, the oven temperature is 68℃.

[0134] 12) Second intermediate rolling

[0135] The milling process was continued until 1.5 mm and the processing rate was controlled at 46.43%.

[0136] 13) The third high temperature heat treatment

[0137] The bell-type furnace annealing was adopted, and the protective atmosphere was a reducing atmosphere of 78% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 540℃ at a heating rate of 127℃ / h and keep it at that temperature for 5.2h, and then cool it to room temperature at a rate of 76℃ / h. The average grain size is controlled at 93μm.

[0138] 14) Cleaning

[0139] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 8.3, and the solution temperature is 64°C; then pickling is performed, the sulfuric acid concentration is 123g / l, the temperature is 35°C, and the Cu in the acid solution is 2+ ≤1.2g / l; clean and dry, the oven temperature is 66℃.

[0140] 15) Finished product rolling

[0141] The finished product is rolled to 0.8mm, and the processing rate is controlled at 46.66%.

[0142] 16) Finished product heat treatment

[0143] The bell-type furnace annealing was adopted, and the protective atmosphere was a reducing atmosphere of 77% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 475℃ at a heating rate of 128℃ / h and keep it at this temperature for 5.7h, and then cool it to room temperature at a rate of 85℃ / h. The average grain size of the finished product is controlled at 80μm.

[0144] 17) Cleaning

[0145] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 8.1, and the solution temperature is 66°C; then pickling is performed, the sulfuric acid concentration is 124g / l, the temperature is 36°C, and the Cu in the acid solution is 2+ ≤1.2g / l; cleaning and drying, the oven temperature is 68℃, during the cleaning process, the tension between the unwinding and pickling S roller group and the winding tension are controlled at 8N / mm 2 .

[0146] 18) Finished products are striped and packaged.

[0147] Example 3

[0148] The preparation steps of the copper alloy strip of this embodiment are as follows:

[0149] 1) Ingredient smelting + aeration and impurity removal

[0150] Add electrolytic copper to the smelting furnace to heat and melt, then raise the temperature to 1135℃, use the bottom blowing generator of the smelting furnace to blow in compressed air, the blowing flow rate is 15L / min, the pressure is 0.04MPa, the blowing time is 37min, wait for the copper liquid to be still for 11min, and then remove the oxide slag. After oxygenation and impurity removal, the impurity elements are controlled at P<0.0005wt%%,Si<0.001wt%%,Al<0.0005wt%%,Sn<0.001wt%%,Mg<0.0005wt%%%,Fe<0.001wt%%%,Ni<0.001wt%%。Then add zinc ingots according to the composition ratio, keep warm for 20 to 30 minutes, then remove the slag, and start casting.

[0151] 2) Semi-continuous casting of red ingots

[0152] The temperature of the copper liquid is controlled at 1114℃, the frequency of the vibrator is 43 times / min, the amplitude is 4.8mm, the crystallizer is covered with anhydrous borax during the entire casting process, and the casting speed of the ingot is 67mm / min. The crystallizer adopts primary cooling without secondary cooling, and the primary cooling water flow is 42m 3 / h, water pressure 0.52MPa, water inlet temperature 24℃, water outlet temperature controlled at 44℃, ingot temperature out of crystallizer at 660℃, then air-cooled to below 80℃ for 36 hours, ingot drawing specification is 230*620mm*8000mm.

[0153] 3) Hot rolling + online heat treatment

[0154] The ingot heating temperature is 865℃, the holding time is 2.6h, the hot rolling starting temperature is 835℃, hot rolling is carried out to a thickness of 12mm, and the hot rolling final rolling temperature is ensured to be 580℃, and the width of the hot rolling widened strip is 650±5mm. After the hot rolling final rolling material temperature drops to 550℃, the hot-rolled strip is coiled online and placed in the heat treatment furnace within 10 minutes, and the heat treatment furnace temperature is adjusted to 600℃, kept warm for 2.2 hours, and then air-cooled to below 80℃, and the average grain size is controlled at 164μm.

[0155] 4) Milling

[0156] The single-sided milling amount is 0.75mm, and the milling surface is 10.5mm thick.

[0157] 5) Rough rolling

[0158] Rough rolling to 5mm, the processing rate is controlled at 52.38%.

[0159] 6) Trimming

[0160] The single-side shearing is 7-10mm, and the belt width after shearing is 630±0.5mm.

[0161] 7) First high temperature heat treatment

[0162] The bell-type furnace annealing was adopted, and the protective atmosphere was a reducing atmosphere of 74% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 585℃ at a heating rate of 140℃ / h and keep it at that temperature for 4.9h, and then cool it to room temperature at a rate of 80℃ / h. The average grain size is controlled at 128μm.

[0163] 8) Cleaning

[0164] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 8.3, and the solution temperature is 68°C; then pickling is performed, the sulfuric acid concentration is 124g / l, the temperature is 35°C, and the Cu in the acid solution is 2+ ≤1.2g / l; clean and dry, the oven temperature is 69℃.

[0165] 9) First intermediate rolling

[0166] Medium rolling to 2.5mm, processing rate 50%.

[0167] 10) Second high temperature heat treatment

[0168] The bell-type furnace annealing was adopted, and the protective atmosphere was a reducing atmosphere of 76% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 555℃ at a heating rate of 117℃ / h and keep it at that temperature for 5.3h, and then cool it to room temperature at a rate of 72℃ / h. The average grain size is controlled at 96μm.

[0169] 11) Cleaning

[0170] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 8.4, and the solution temperature is 67°C; then pickling is performed, the sulfuric acid concentration is 119g / l, the temperature is 33°C, and the Cu in the acid solution is 2+ ≤1.2g / l; clean and dry, the oven temperature is 68℃.

[0171] 12) Second intermediate rolling

[0172] Medium rolling to 1.45mm, the processing rate is controlled at 44%.

[0173] 13) The third high temperature heat treatment

[0174] The bell-type furnace annealing was adopted, and the protective atmosphere was a reducing atmosphere of 76% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 549℃ at a heating rate of 124℃ / h and keep it at this temperature for 5.8h, and then cool it to room temperature at a rate of 82℃ / h. The average grain size is controlled at 89μm.

[0175] 14) Cleaning

[0176] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 8, and the solution temperature is 64°C; then pickling is performed, the sulfuric acid concentration is 124g / l, the temperature is 36°C, and the Cu in the acid solution is 2+ ≤1.2g / l; clean and dry, the oven temperature is 69℃.

[0177] 15) Finished product rolling

[0178] The finished product is rolled to 0.75mm and the processing rate is controlled at 48.28%.

[0179] 16) Finished product heat treatment

[0180] The bell-type furnace annealing was adopted, and the protective atmosphere was a reducing atmosphere of 77% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 465℃ at a heating rate of 136℃ / h and keep it at that temperature for 4.9h, and then cool it to room temperature by air cooling at a rate of 75℃ / h. The average grain size of the finished product is controlled at 75μm.

[0181] 17) Cleaning

[0182] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 7.8, and the solution temperature is 67°C; then pickling is performed, the sulfuric acid concentration is 116g / l, the temperature is 37°C, and the Cu in the acid solution is 2+ ≤1.2g / l; cleaning and drying, the oven temperature is 67℃, during the cleaning process, the tension between the unwinding and pickling S roller group and the winding tension are controlled at 7.0N / mm 2 .

[0183] 18) Finished products are striped and packaged.

[0184] Example 4

[0185] The preparation steps of the copper alloy strip of this embodiment are as follows:

[0186] 1) Ingredient smelting + aeration and impurity removal

[0187] Add electrolytic copper to the smelting furnace to heat and melt, then raise the temperature to 1127℃, use the bottom blowing generator of the smelting furnace to blow in compressed air, the blowing flow rate is 14L / min, the pressure is 0.055MPa, the blowing time is 34min, wait for the copper liquid to stand for 14min, and then remove the oxide slag. After oxygenation and impurity removal, the impurity elements are controlled at P<0.0005wt%%,Si<0.001wt%%,Al<0.0005wt%%,Sn<0.001wt%%,Mg<0.0005wt%%%,Fe<0.001wt%%%,Ni<0.001wt%%。Then add zinc ingots according to the composition ratio, keep warm for 20 to 30 minutes, then remove the slag, and start casting.

[0188] 2) Semi-continuous casting of red ingots

[0189] The temperature of the copper liquid is controlled at 1114℃, the frequency of the vibrator is 42 times / min, the amplitude is 5.3mm, the crystallizer is covered with anhydrous borax during the entire casting process, and the casting speed of the ingot is 61mm / min. The crystallizer adopts primary cooling without secondary cooling, and the primary cooling water flow is 39m 3 / h, water pressure 0.46MPa, water inlet temperature 22℃, water outlet temperature controlled at 43℃, ingot temperature out of crystallizer at 640℃, then air-cooled to below 80℃ for 36 hours, ingot drawing specification is 230*620mm*8000mm.

[0190] 3) Hot rolling + online heat treatment

[0191] The ingot heating temperature is 865℃, the holding time is 2.4h, the hot rolling starting temperature is 834℃, hot rolling is to 12mm thick, and the hot rolling final rolling temperature is 578℃, and the width of the hot rolling widening is 650±5mm. After the hot rolling final rolling material temperature drops to 550℃, the hot rolled strip is coiled online and placed in the heat treatment furnace within 10 minutes, and the heat treatment furnace temperature is adjusted to 602℃, kept warm for 2.3 hours, and then air cooled to below 80℃, and the average grain size is controlled at 165μm.

[0192] 4) Milling

[0193] The single-sided milling amount is 0.75mm, and the milling surface is 10.5mm thick.

[0194] 5) Rough rolling

[0195] Rough rolling to 4.5mm, processing rate 57.14%.

[0196] 6) Trimming

[0197] The single-side shearing is 7-10mm, and the belt width after shearing is 630±0.5mm.

[0198] 7) First high temperature heat treatment

[0199] The bell-type furnace annealing was adopted, and the protective atmosphere was a reducing atmosphere of 74% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 575℃ at a heating rate of 135℃ / h and keep it at that temperature for 5.5h, and then cool it to room temperature at a rate of 75℃ / h. The average grain size is controlled at 129μm.

[0200] 8) Cleaning

[0201] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 8.1, and the solution temperature is 64°C; then pickling is performed, the sulfuric acid concentration is 116g / l, the temperature is 35°C, and the Cu in the acid solution is 2+ ≤1.2g / l; clean and dry, the oven temperature is 68℃.

[0202] 9) First intermediate rolling

[0203] Medium rolling to 2.5mm, processing rate 44.44%.

[0204] 10) Second high temperature heat treatment

[0205] The bell-type furnace annealing was adopted, and the protective atmosphere was a reducing atmosphere of 72% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 562℃ at a heating rate of 127℃ / h and keep it at this temperature for 5.3h, and then cool it to room temperature at a rate of 81℃ / h. The average grain size is controlled at 98μm.

[0206] 11) Cleaning

[0207] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 7.9, and the solution temperature is 64°C; then pickling is performed, the sulfuric acid concentration is 117g / l, the temperature is 36°C, and the Cu content in the acid is 2+ ≤1.2g / l; clean and dry, the oven temperature is 66℃.

[0208] 12) Second intermediate rolling

[0209] Medium rolling to 1.2mm, processing rate 52%.

[0210] 13) The third high temperature heat treatment

[0211] The bell-type furnace annealing was adopted, and the protective atmosphere was a reducing atmosphere of 76% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 537℃ at a heating rate of 124℃ / h and keep it at that temperature for 4.8h, and then cool it to room temperature at a rate of 72℃ / h. The average grain size is controlled at 96μm.

[0212] 14) Cleaning

[0213] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 8.4, and the solution temperature is 68°C; then pickling is performed, the sulfuric acid concentration is 122g / l, the temperature is 37°C, and the Cu in the acid solution is 2+ ≤1.2g / l; clean and dry, the oven temperature is 69℃.

[0214] 15) Finished product rolling

[0215] The finished product is rolled to 0.6mm and the processing rate is controlled at 50%.

[0216] 16) Finished product heat treatment

[0217] The bell-type furnace annealing was adopted, and the protective atmosphere was a reducing atmosphere of 75% H 2 + balance nitrogen mixed gas. The heat treatment process is to first heat the alloy copper strip to 472℃ at a heating rate of 130℃ / h and keep it at that temperature for 4.4h, and then cool it to room temperature at a rate of 80℃ / h. The average grain size of the finished product is controlled at 81μm.

[0218] 17) Cleaning

[0219] First, degreasing is performed, and the degreasing agent is sodium hydroxide aqueous solution, the pH range is 8.5, and the solution temperature is 62°C; then pickling is performed, the sulfuric acid concentration is 120g / l, the temperature is 32°C, and the Cu in the acid solution is 2+ ≤1.2g / l; cleaning and drying, the oven temperature is 67℃, during the cleaning process, the tension between the unwinding and pickling S roller group and the winding tension are controlled at 7.5N / mm 2 .

[0220] 18) Finished products are striped and packaged.

[0221] Comparative Example 1

[0222] The copper alloy strip of this embodiment contains the following mass percentages: 65.2% Cu, the remainder Zn. The preparation steps are different from those of Example 4 in that: Step 1) ingredients are smelted without aeration and impurity removal process, i.e., compressed air is not blown in.

[0223] Comparative Example 2

[0224] The copper alloy strip of this embodiment contains the following mass percentages: Cu65.2%, and the balance is Zn. The preparation steps are different from those of embodiment 4 in that: Step 3) hot rolling, no online heat treatment process, that is, the hot rolling final material temperature drops to 550°C and then is directly coiled and cooled.

[0225] Comparative Example 3

[0226] The copper alloy strip of this embodiment contains the following mass percentage of element Cu65.2%, and the balance is Zn. The preparation steps are different from those of Example 4 in that the processing rate of step 5) rough rolling and step 9) first intermediate rolling is 66.66%, that is, the rough rolling to 3.5mm, the first intermediate rolling to 1.166mm, and the finished product rolling to 0.6mm is 48.54%. Due to the rough rolling, the first intermediate rolling and the finished product processing rate, the second intermediate rolling has no room for cold working, so the comparative example 3 does not have step 12) second intermediate rolling, step 13) third high temperature heat treatment and step 14) cleaning process.

[0227] The mechanical properties, electrical conductivity, and organizational structure of the copper alloy strips prepared in Examples 1 to 4 and Comparative Examples 1 to 3 were tested, and the results are shown in Table 4. The test method is as follows:

[0228] Mechanical properties testing: The room temperature tensile test is carried out on an electronic universal mechanical properties testing machine in accordance with GB / T 228.1-2010 Tensile test of metallic materials Part 1: Room temperature test method, using a 20mm wide headed specimen and a tensile speed of 15mm / min.

[0229] Metallographic structure grain size test: According to the interception method in GB / T 6394-2007 Metal Average Grain Size Determination Method, the grain size in the photo collected by 100 times metallographic microscope is tested. The sample width is 10mm and the length is 10mm.

[0230] The copper alloy finished strips prepared in Examples 1 to 4 have a hardness of <56 HV, a tensile strength of <260 MPa, an elongation of >55%, and a finished grain size of 60 to 90 μm. They have extremely low strength and excellent elongation, good plasticity, meet the rolling composite performance requirements of copper-steel composite strips, and can be used to produce copper-steel composite strips for bullets.

[0231] Table 2 Chemical composition of the copper alloy strips of various embodiments of the present invention and comparative examples (wt%)

[0232] serial number Cu Zn and inevitable impurities Example 1 63.95 margin Example 2 64.5 margin Example 3 65.4 margin Example 4 65.2 margin Comparative Example 1 65.2 margin Comparative Example 2 65.2 margin Comparative Example 3 65.2 margin

[0233] Table 3 Key process parameter control of various embodiments of the present invention and comparative examples

[0234]

[0235] Table 4 Organization structure and performance of various embodiments of the present invention and comparative examples

[0236]

[0237] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a brass strip, characterized in that: The following steps are involved: Ingredient smelting + gasification and impurity removal → semi-continuous casting red ingot casting → hot rolling + online heat treatment → rough rolling → first heat treatment → first intermediate rolling → second heat treatment → second intermediate rolling → third heat treatment → finished product rolling → finished product heat treatment; Among them, in the batch smelting + charging and de-impurity process, the raw material ratio satisfies Cu: 63.5-66wt%, and the balance is Zn and unavoidable impurities; the conditions for charging and de-impurity are: blowing compressed air into the smelting furnace, the blowing flow rate is 10-20L / min, the pressure is 0.02-0.1MPa, and the blowing time is 20-40min.

2. The preparation method according to claim 1, characterized in that: In the hot rolling + online heat treatment process, the hot rolling start temperature is 820-850°C, the hot rolling final rolling temperature is above 550°C, and after the hot rolling final rolling material temperature drops to 550°C, the hot-rolled strip is coiled online and placed in a heat treatment furnace within 10 minutes, and the temperature of the heat treatment furnace is adjusted to 580-610°C and kept warm for 2-3 hours.

3. The preparation method according to claim 1, characterized in that: The rough rolling processing rate, the first intermediate rolling processing rate and the second intermediate rolling processing rate are controlled at 40-60%, and the finished product rolling processing rate is controlled at 45-55%.

4. The preparation method according to claim 1, characterized in that: In the first heat treatment, the second heat treatment and the third heat treatment process, the alloy copper strip is heated to 550-600° C., 540-580° C. and 520-560° C. respectively, and kept warm for 4-6 hours.

5. The preparation method according to claim 1, characterized in that: In the finished product heat treatment process, the alloy copper strip is heated to 450-480° C. and kept warm for 4-6 hours.

6. The preparation method according to claim 1, characterized in that: The alloy copper strip is cleaned after the first heat treatment, the second heat treatment, the third heat treatment and the finished product heat treatment. During the cleaning process, the middle tension of the unwinding and pickling S roller group and the winding tension are controlled at 10N / mm 2 Within.

7. The brass strip prepared by the preparation method according to any one of claims 1 to 6.

8. The brass strip according to claim 7, characterized in that The brass strip has a hardness of less than 56 HV, a tensile strength of less than 260 MPa, and an elongation of more than 55%.

9. The preparation method according to claim 7 or 8, characterized in that: The average grain size of the brass strip is 60-90 μm.

10. Use of the brass strip according to any one of claims 7 to 9 in preparing copper-steel composite strips for bullet casings.

Citation Information

Cited By