Preparation method of large-size TC20 titanium alloy cast ingot

By using AlNb binary alloy and reasonable vacuum consumable smelting process in the preparation of TC20 titanium alloy ingots, the problem of Nb element segregation is solved, and the composition uniformity and high performance of large-scale ingots are achieved, which is suitable for industrial production.

CN118932204APending Publication Date: 2024-11-12WESTERN TITANIUM TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411032245.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is prone to segregation defects of Nb elements when preparing TC20 titanium alloy ingots, and the cooling rate slows down after the ingot specifications are increased, further increasing the segregation degree of Nb elements, making it difficult to eliminate macroscopic segregation defects through subsequent hot processing. Impact subsequent processing performance.

Method used

Add Nb elements by adding AlNb binary alloy, and design a reasonable vacuum self-consumption smelting process, including multiple smelting processes, control smelting parameters such as voltage, current and vacuum degree, ensure uniformity of ingot components, and avoid Nb elements. Semi-analysis.

Benefits of technology

The composition uniformity of large-scale TC20 titanium alloy ingots is achieved, the macroscopic and micro-zone segregation of Nb elements is avoided, the processing performance of the material is improved, and the application range is wide and easy to be produced in industrial form.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932204A_ABST
    Figure CN118932204A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a large-size TC20 titanium alloy cast ingot. The preparation method comprises the following steps: 1, selecting sponge titanium, an AlNb binary alloy, aluminum shots and titanium dioxide as raw materials; 2, weighing and uniformly mixing the selected raw materials to obtain a raw material mixture; 3, pressing the raw material mixture into a plurality of electrode blocks, and welding to obtain a consumable electrode; and fourthly, the consumable electrode is smelted, and the large-specification TC20 titanium alloy cast ingot is obtained. According to the method, the Nb element is added in a mode of adding the AlNb binary alloy, the smelting parameters are reasonably designed, the smelted cast ingot does not have macroscopic and microcell composition segregation of the Nb element, the problems existing in TC20 titanium alloy cast ingot preparation can be effectively solved, the prepared large-size TC20 titanium alloy cast ingot is uniform in composition, the diameter is not smaller than 640 mm, and the yield is high. The problems existing in TC20 titanium alloy cast ingot preparation are effectively solved, and the method is reasonable in design, easy to operate, wide in application range and easy for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of TC20 titanium alloy preparation, and in particular relates to a method for preparing a large-size TC20 titanium alloy ingot. Background Art

[0002] TC20 (Ti6Al7Nb) titanium alloy is mainly composed of three elements: titanium, aluminum and niobium. Sometimes iron, oxygen and other elements are added to it to enhance performance. TC20 titanium alloy has excellent mechanical properties, corrosion resistance and biocompatibility. It is a high-performance material widely used in medical and industrial technology fields.

[0003] Conventional TC20 titanium alloy semi-finished products are bars or plates. Its production process is: sponge titanium / intermediate alloy mixing → pressing electrodes and welding → vacuum consumable melting → bar / plate forging. Since TC20 titanium alloy contains 7wt.% Nb element, its density is 8.57g / cm 3 , significantly higher than Ti (4.5g / cm 3 ) and Al(2.7g / cm 3 ) element density. Therefore, if the conventional method is used to prepare TC20 titanium alloy ingots by vacuum consumable smelting, segregation defects of Nb elements are likely to occur; at the same time, after the ingot specifications are increased, the cooling rate of the ingot solidification process slows down, further increasing the segregation degree of Nb elements in the ingot. Macro segregation defects cannot be eliminated by subsequent hot working and heat treatment, and they will be inherited to bars and plates, seriously affecting their subsequent processing and use performance.

[0004] Therefore, it is necessary to provide a method for preparing a TC20 titanium alloy ingot with uniform composition and no macroscopic and microscopic composition segregation of the Nb element. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for preparing a large-sized TC20 titanium alloy ingot in view of the deficiencies of the above-mentioned prior art. The method adds the Nb element by adding an AlNb binary alloy, and through a reasonably designed smelting process, the prepared large-sized TC20 titanium alloy ingot has uniform composition and no macroscopic and micro-region composition segregation of the Nb element, which can effectively solve the problems existing in the preparation of the TC20 titanium alloy ingot. The method has a reasonable design, simple operation, a wide range of application, and is easy to industrialize.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a large-size TC20 titanium alloy ingot, characterized in that the method comprises the following steps:

[0007] Step 1: Raw material selection: titanium sponge, AlNb binary alloy, aluminum beans and titanium dioxide are selected as raw materials;

[0008] Step 2: Mixing: weighing and mixing the raw materials selected in step 1 to obtain a raw material mixture;

[0009] Step 3: preparing electrode blocks: pressing the raw material mixture obtained in step 2 into a plurality of electrode blocks, and welding the plurality of electrode blocks in a vacuum plasma welding box to obtain consumable electrodes;

[0010] Step 4: Smelt the consumable electrode obtained in step 3 in a vacuum consumable arc furnace to obtain a large-sized TC20 titanium alloy ingot, wherein the diameter of the ingot is not less than 640 mm.

[0011] The above-mentioned method for preparing a large-size TC20 titanium alloy ingot is characterized in that the sponge titanium in step 1 is above grade 1, and the mass content of Ti is not less than 99.6%. The present invention prevents the introduction of impurities by controlling the grade of the sponge titanium and the content of Ti, thereby improving the performance of the TC20 titanium alloy ingot.

[0012] The above-mentioned method for preparing a large-size TC20 titanium alloy ingot is characterized in that the AlNb binary alloy in step 1 is AlNb60 or AlNb70, and the particle size is not greater than 0.5 mm. In the present invention, AlNb60 or AlNb70 is used as the raw material of Nb. The melting point of AlNb60 or AlNb70 is much lower than the melting point of Nb, which is closer to Ti, and is more conducive to its alloying, preventing the deficiency of too high a smelting temperature when Nb is added. At the same time, controlling the particle size will also be more conducive to its alloying, preventing the particle size from being too large, which is not conducive to its complete melting and has the risk of the existence of unmelted blocks.

[0013] The above-mentioned method for preparing a large-size TC20 titanium alloy ingot is characterized in that, in the welding described in step 3, both the longitudinal and transverse surfaces of the electrode block are welded, and the weld width is not less than 20 mm. The present invention performs welding on both the longitudinal and transverse surfaces of the electrode block and controls the weld width, so that the consumable electrode has a certain strength, avoids welding only one surface or the weld width is too narrow, and there is a risk of falling off during one smelting.

[0014] The above-mentioned method for preparing a large-size TC20 titanium alloy ingot is characterized in that the smelting in step 4 specifically includes the following steps:

[0015] Step 401, primary smelting: smelting the consumable electrode prepared in step 3 to obtain a primary ingot;

[0016] Step 402, secondary smelting: performing secondary smelting on the primary ingot obtained in step 401 to obtain a secondary ingot;

[0017] Step 403, three smelting: the secondary ingot obtained in step 402 is smelted three times to obtain a large-size, high-homogeneity TC20 titanium alloy ingot. The present invention performs three smeltings, the main purpose of the first smelting is to fully alloy and remove impurities; the main purpose of the second smelting is to further remove impurities and initially ensure uniform composition; the main purpose of the third smelting is to ensure uniform composition of the ingot.

[0018] The above-mentioned method for preparing a large-size TC20 titanium alloy ingot is characterized in that the crucible diameter used in the first smelting in step 401 is 500mm-640mm, the smelting voltage is 31V-38V, the smelting current is 10kA-20kA, the arc stabilization current is 5A-22A, the arc stabilization period is 0-25s, the vacuum degree is below 10Pa, and the cooling time in the furnace after the smelting is completed is not less than 280min. The present invention controls the parameters of the first smelting to fully alloy the raw materials, remove impurities from the raw materials, and improve the uniformity of the TC20 titanium alloy ingot.

[0019] The above-mentioned method for preparing a large-size TC20 titanium alloy ingot is characterized in that the crucible diameter used in the secondary smelting in step 402 is 560mm-720mm, the smelting voltage is 31V-36V, the smelting current is 15kA-27kA, the arc stabilization current is 5A-25A, the arc stabilization period is 5s-30s, the vacuum degree is below 5Pa, and the cooling time in the furnace after the smelting is completed is not less than 310min. The present invention further removes impurities by controlling the parameters of the secondary smelting, preliminarily ensures uniform composition, and improves the uniformity of the TC20 titanium alloy ingot.

[0020] The above-mentioned method for preparing a large-size TC20 titanium alloy ingot is characterized in that the crucible diameter used in the three smeltings in step 403 is 640mm-820mm, the smelting voltage is 31V-36V, the smelting current is 17kA-30kA, the arc stabilization current is 10A-30A, the arc stabilization period is 5s-30s, the vacuum degree is below 3Pa, and the cooling time in the furnace after the smelting is completed is not less than 350min. The present invention ensures that the composition of the TC20 titanium alloy ingot is uniform by controlling the parameters of the three smeltings.

[0021] The above-mentioned method for preparing a large-size TC20 titanium alloy ingot is characterized in that, in the three smeltings described in step 403, when the remaining mass of the secondary ingot is 3% to 8% of the original mass of the secondary ingot, the shrinkage compensation is started, and the shrinkage compensation process is: gradually reducing the smelting current, smelting voltage and arc stabilization current, so that the molten pool gradually becomes shallower, and when the smelting current is reduced to 4kA, it is maintained for more than 30 minutes. The present invention obtains a shallower riser by controlling the shrinkage compensation parameters, thereby reducing the riser removal amount, improving the yield rate, and reducing production costs.

[0022] Compared with the prior art, the present invention has the following advantages:

[0023] 1. The present invention adds the Nb element by adding AlNb binary alloy, thereby avoiding the possibility of unalloying due to the high melting point when pure Nb is added, and combines smelting to obtain a large-sized TC20 titanium alloy ingot with a diameter of not less than 640 mm.

[0024] 2. The present invention realizes the preparation of large-sized TC20 titanium alloy ingots by optimizing the raw material types and formulating reasonable vacuum consumable smelting parameters. The method has simple steps, reasonable design, easy industrial production and good use effect. The prepared large-sized titanium alloy ingots have uniform composition and no segregation defects.

[0025] 3. The present invention has a wide application range and is easy for industrial production. The ingot shape of the three-smelting ingot gradually increases, which is more conducive to industrial mass production.

[0026] 4. The technical solution proposed in the present invention is simple, reasonably designed, widely applicable and easy to industrialize. The prepared large-scale TC20 titanium alloy ingots have uniform composition, no macro- and micro-region composition segregation of the Nb element, and can effectively solve the problems existing in the preparation of large-scale TC20 titanium alloy ingots.

[0027] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a Nb content distribution diagram of the riser cross section of the large-scale and highly homogeneous TC20 titanium alloy ingot prepared in Example 1 of the present invention.

[0029] Figure 2 This is the Nb content distribution diagram of the riser cross section of the large-scale and highly homogeneous TC20 titanium alloy ingot prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0030] Example 1

[0031] This embodiment includes the following steps:

[0032] Step 1: Raw material selection: select grade 0 titanium sponge with a particle size of 0.83 mm to 25.4 mm, AlNb60 binary alloy with a particle size not greater than 0.5 mm, aluminum beans, titanium dioxide and ferro-titanium alloy;

[0033] Step 2, mixing: weigh the raw materials selected in step 1 according to Ti-6Al-7Nb-0.2O-0.2Fe to obtain 3000 kg of raw materials, and then divide the raw materials into 50 portions, mix them in a fully automatic mixing system, and the number of rotations of the mixer is greater than 10 circles, to obtain 50 portions of raw material mixture;

[0034] Step 3, electrode block preparation: 50 portions of the raw material mixture obtained in step 2 are respectively pressed into 50 electrode blocks at a pressure of not less than 3500 MPa, and the longitudinal and transverse surfaces of the 50 electrode blocks are welded in a vacuum plasma welding box, and the weld width is not less than 20 mm, to obtain a consumable electrode with no burrs on the surface;

[0035] Step 4: Smelting the consumable electrode obtained in step 3 in a vacuum consumable arc furnace to obtain a large-sized and highly homogeneous TC20 titanium alloy ingot;

[0036] The smelting specifically comprises the following steps:

[0037] Step 401, primary smelting: the consumable electrode prepared in step 3 is smelted once to obtain a primary ingot; the crucible diameter used in the primary smelting is 500 mm, the smelting voltage is 31V-38V, the smelting current is 10kA-14kA, the arc stabilizing current is 5A-20A, the arc stabilizing period is 0-25s, the vacuum degree is below 10Pa, and the cooling time in the furnace after the smelting is completed is not less than 280min;

[0038] Step 402, secondary smelting: the primary ingot obtained in step 401 is subjected to secondary smelting to obtain a secondary ingot; the crucible diameter used in the secondary smelting is 560 mm, the smelting voltage is 31V-36V, the smelting current is 15kA-21kA, the arc stabilizing current is 5A-25A, the arc stabilizing period is 5s-30s, the vacuum degree is below 5Pa, and the cooling time in the furnace after the smelting is completed is not less than 310min;

[0039] Step 403, three smeltings: the secondary ingot obtained in step 402 is smelted three times to obtain a large-size, high-homogeneity TC20 titanium alloy ingot; the crucible diameter used for the three smeltings is 640 mm, the smelting voltage is 31V-36V, the smelting current is 17kA-25kA, the arc stabilization current is 10A-30A, the arc stabilization period is 5s-30s, the vacuum degree is below 3Pa, and the cooling time in the furnace after the smelting is not less than 350min; in the three smeltings, when the residual mass of the secondary ingot is 8% of the original mass, shrinkage compensation is started, and the smelting current, smelting voltage and arc stabilization current are gradually reduced to make the molten pool gradually shallower, and when the smelting current is reduced to 4kA, it is maintained for more than 30min.

[0040] Figure 1 This is the Nb content distribution diagram of the riser cross section of the large-scale, highly homogeneous TC20 titanium alloy ingot prepared in this embodiment. Figure 1100-1, 100-2, 100-3, 100-4 in the horizontal axis represent that 4 samples are taken at a distance of 100 mm from the center of the TC20 titanium alloy ingot riser, and the positions of the 4 samples are each spaced 90° apart; 200-1, 200-2, 200-3, 200-4 represent that 4 samples are taken at a distance of 200 mm from the center of the TC20 titanium alloy ingot riser, and the positions of the 4 samples are each spaced 90° apart; 300-1, 300-2, 300-3, 300-4 represent that 4 samples are taken at a distance of 300 mm from the center of the TC20 titanium alloy ingot riser, and the positions of the 4 samples are each spaced 90° apart. Figure 1 It can be seen that there is no macro segregation of Nb element in the riser part.

[0041] According to tests, the large-scale, highly homogeneous TC20 titanium alloy ingot prepared in this embodiment has a diameter of up to 640 mm, a mass of up to 3000 kg, a uniform composition, and no macroscopic segregation of the Nb element.

[0042] Example 2

[0043] This embodiment includes the following steps:

[0044] Step 1: Raw material selection: select grade 0 titanium sponge with a particle size of 0.83 mm to 25.4 mm, AlNb60 binary alloy with a particle size not greater than 0.5 mm, aluminum beans, and titanium dioxide;

[0045] Step 2, mixing: weigh the raw materials selected in step 1 according to Ti-6Al-7Nb to obtain 3000 kg of raw materials, then divide the raw materials into 50 parts, mix them in a fully automatic mixing system, and the number of rotations of the mixer is greater than 10 circles, to obtain 50 parts of raw material mixture;

[0046] Step 3, electrode block preparation: 50 portions of the raw material mixture obtained in step 2 are respectively pressed into 50 electrode blocks at a pressure of not less than 3500 MPa, and the longitudinal and transverse surfaces of the 50 electrode blocks are welded in a vacuum plasma welding box, and the weld width is not less than 20 mm, to obtain a consumable electrode with no burrs on the surface;

[0047] Step 4: Smelting the consumable electrode obtained in step 3 in a vacuum consumable arc furnace to obtain a large-sized and highly homogeneous TC20 titanium alloy ingot;

[0048] The smelting specifically comprises the following steps:

[0049] Step 401, primary smelting: the consumable electrode prepared in step 3 is smelted once to obtain a primary ingot; the crucible diameter used in the primary smelting is 560 mm, the smelting voltage is 31V-38V, the smelting current is 12kA-18kA, the arc stabilizing current is 5A-20A, the arc stabilizing period is 0-25s, the vacuum degree is below 10Pa, and the cooling time in the furnace after the smelting is completed is not less than 310min;

[0050] Step 402, secondary smelting: the primary ingot obtained in step 401 is subjected to secondary smelting to obtain a secondary ingot; the crucible diameter used in the secondary smelting is 640 mm, the smelting voltage is 31V-36V, the smelting current is 19kA-27kA, the arc stabilizing current is 5A-25A, the arc stabilizing period is 5s-30s, the vacuum degree is below 5Pa, and the cooling time in the furnace after the smelting is completed is not less than 350min;

[0051] Step 403, three smeltings: the secondary ingot obtained in step 402 is smelted three times to obtain a large-size, high-homogeneity TC20 titanium alloy ingot; the crucible diameter used for the three smeltings is 720 mm, the smelting voltage is 31V-36V, the smelting current is 20kA-30kA, the arc stabilization current is 10A-30A, the arc stabilization period is 5s-30s, the vacuum degree is below 3Pa, and the cooling time in the furnace after the smelting is not less than 410min; in the three smeltings, when the residual mass of the secondary ingot is 5% of the original mass, shrinkage compensation is started, and the smelting current, smelting voltage and arc stabilization current are gradually reduced to make the molten pool gradually shallower, and when the smelting current is reduced to 4kA, it is maintained for more than 30min.

[0052] Figure 2 This is the Nb content distribution diagram of the riser cross section of the large-scale, highly homogeneous TC20 titanium alloy ingot prepared in this embodiment. Figure 2 The 180-1 and 180-2 in the horizontal axis indicate that two samples are taken at a distance of 180 mm from the center of the TC20 titanium alloy ingot riser, and the interval between the two samples is 180°. The 360-1 and 360-2 indicate that two samples are taken at a distance of 360 mm from the center of the TC20 titanium alloy ingot riser, and the interval between the two samples is 180°. Figure 2 It can be seen that there is no macro segregation of Nb element in the riser part.

[0053] According to tests, the large-scale, highly homogeneous TC20 titanium alloy ingot prepared in this embodiment has a diameter of up to 720 mm, a mass of up to 3000 kg, a uniform composition, and no macroscopic segregation of the Nb element.

[0054] Example 3

[0055] This embodiment includes the following steps:

[0056] Step 1: Raw material selection: select grade 0 titanium sponge with a particle size of 0.83 mm to 25.4 mm, AlNb70 binary alloy with a particle size not greater than 0.5 mm, aluminum beans, and titanium dioxide;

[0057] Step 2, mixing: weigh the raw materials selected in step 1 according to Ti-6.2Al-6.8Nb-0.18O to obtain 6000 kg of raw materials, and then divide the raw materials into 40 parts, mix them in a fully automatic mixing system, and the number of rotations of the mixer is greater than 10 circles, to obtain 40 parts of raw material mixture;

[0058] Step 3, electrode block preparation: 40 portions of the raw material mixture obtained in step 2 are respectively pressed into 40 electrode blocks at a pressure of not less than 3500 MPa, and the longitudinal and transverse surfaces of the 40 electrode blocks are welded in a vacuum plasma welding box, and the weld width is not less than 20 mm, to obtain a consumable electrode with no burrs on the surface;

[0059] Step 4: Smelting the consumable electrode obtained in step 3 in a vacuum consumable arc furnace to obtain a large-sized and highly homogeneous TC20 titanium alloy ingot;

[0060] The smelting specifically comprises the following steps:

[0061] Step 401, primary smelting: the consumable electrode prepared in step 3 is smelted once to obtain a primary ingot; the crucible diameter used in the primary smelting is 640 mm, the smelting voltage is 31V-38V, the smelting current is 15kA-20kA, the arc stabilizing current is 8A-22A, the arc stabilizing period is 0-25s, the vacuum degree is below 10Pa, and the cooling time in the furnace after the smelting is completed is not less than 280min;

[0062] Step 402, secondary smelting: the primary ingot obtained in step 401 is subjected to secondary smelting to obtain a secondary ingot; the crucible diameter used in the secondary smelting is 720 mm, the smelting voltage is 31V-36V, the smelting current is 20kA-24kA, the arc stabilizing current is 10A-25A, the arc stabilizing period is 10s-30s, the vacuum degree is below 5Pa, and the cooling time in the furnace after the smelting is completed is not less than 310min;

[0063] Step 403, three smeltings: the secondary ingot obtained in step 402 is smelted three times to obtain a large-size, high-homogeneity TC20 titanium alloy ingot; the crucible diameter used for the three smeltings is 820 mm, the smelting voltage is 31V-36V, the smelting current is 23kA-30kA, the arc stabilization current is 10A-30A, the arc stabilization period is 15s-30s, the vacuum degree is below 3Pa, and the cooling time in the furnace after the smelting is not less than 350min; in the three smeltings, when the residual mass of the secondary ingot is 3% of the original mass, shrinkage compensation is started, and the smelting current, smelting voltage and arc stabilization current are gradually reduced to make the molten pool gradually shallower, and when the smelting current is reduced to 4kA, it is maintained for more than 30min.

[0064] According to tests, the large-scale, highly homogeneous TC20 titanium alloy ingot prepared in this embodiment has a diameter of up to 680 mm, a mass of up to 2000 kg, a uniform composition, and no macroscopic segregation of the Nb element.

[0065] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a large-size TC20 titanium alloy ingot, characterized in that: The method comprises the following steps: Step 1: Raw material selection: titanium sponge, AlNb binary alloy, aluminum beans and titanium dioxide are selected as raw materials; Step 2: Mixing: weighing and mixing the raw materials selected in step 1 to obtain a raw material mixture; Step 3: preparing electrode blocks: pressing the raw material mixture obtained in step 2 into a plurality of electrode blocks, and welding the plurality of electrode blocks in a vacuum plasma welding box to obtain consumable electrodes; Step 4: Smelt the consumable electrode obtained in step 3 in a vacuum consumable arc furnace to obtain a large-sized TC20 titanium alloy ingot, wherein the diameter of the ingot is not less than 640 mm.

2. The method for preparing a large-size TC20 titanium alloy ingot according to claim 1, characterized in that: The titanium sponge described in step 1 is of grade 1 or above, and the mass content of Ti is not less than 99.6%.

3. The method for preparing a large-size TC20 titanium alloy ingot according to claim 1, characterized in that: The AlNb binary alloy in step 1 is AlNb60 or AlNb70, and the particle size is not greater than 0.5 mm.

4. The method for preparing a large-size TC20 titanium alloy ingot according to claim 1, characterized in that: In the welding described in step 3, both the longitudinal and transverse surfaces of the electrode block are welded, and the weld width is not less than 20 mm.

5. The method for preparing a large-size TC20 titanium alloy ingot according to claim 1, characterized in that: The smelting in step 4 specifically includes the following steps: Step 401, primary smelting: smelting the consumable electrode prepared in step 3 to obtain a primary ingot; Step 402, secondary smelting: performing secondary smelting on the primary ingot obtained in step 401 to obtain a secondary ingot; Step 403, tertiary smelting: the secondary ingot obtained in step 402 is smelted tertiary to obtain a large-size and high-homogeneity TC20 titanium alloy ingot.

6. The method for preparing a large-size TC20 titanium alloy ingot according to claim 5, characterized in that: The crucible diameter used for the first smelting in step 401 is 500mm-640mm, the smelting voltage is 31V-38V, the smelting current is 10kA-20kA, the arc stabilization current is 5A-22A, the arc stabilization period is 0-25s, the vacuum degree is below 10Pa, and the cooling time in the furnace after the smelting is completed is not less than 280min.

7. The method for preparing a large-size TC20 titanium alloy ingot according to claim 5, characterized in that: The crucible diameter used for the secondary smelting in step 402 is 560mm-720mm, the smelting voltage is 31V-36V, the smelting current is 15kA-27kA, the arc stabilization current is 5A-25A, the arc stabilization period is 5s-30s, the vacuum degree is below 5Pa, and the cooling time in the furnace after the smelting is completed is not less than 310min.

8. The method for preparing a large-size TC20 titanium alloy ingot according to claim 5, characterized in that: The crucible diameter used for the three smeltings in step 403 is 640mm-820mm, the smelting voltage is 31V-36V, the smelting current is 17kA-30kA, the arc stabilization current is 10A-30A, the arc stabilization period is 5s-30s, the vacuum degree is below 3Pa, and the cooling time in the furnace after the smelting is completed is not less than 350min.

9. The method for preparing a large-size TC20 titanium alloy ingot according to claim 8, characterized in that: In the three smeltings described in step 403, when the remaining mass of the secondary ingot is 3% to 8% of the original mass, shrinkage compensation begins, and the smelting current, smelting voltage and arc stabilization current are gradually reduced to make the molten pool gradually shallower. When the smelting current is reduced to 4kA, it is maintained for more than 30 minutes.

Citation Information

Cited By

  • Ti-Zr-Al alloy and preparation method thereof

    CN119876693A