Heat-free aluminum alloy and preparation method thereof

By adding recycled material containing manganese elements to the aluminum alloy matrix raw material to form (FeMn)Al6 phase, the problems of high cost and low strength of existing recycled aluminum alloy materials are solved, and high strength and low cost heat-free aluminum alloys are achieved Preparation improves its recyclability and supports green closed-loop development.

CN118932205APending Publication Date: 2024-11-12NIO TECH ANHUI CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411042094.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing recycled aluminum alloy materials have high cost and low strength, which cannot meet the high-strength requirements such as new energy vehicle motor shells, and their recyclability is poor, making it difficult to achieve green closed-loop development.

Method used

Using a heat-free aluminum alloy preparation method, the aluminum alloy matrix raw material and the manganese-containing recycled material are melted, alloyed, refined and die-casted to form (FeMn)Al6 phase, reduce the adverse effects of iron and improve the toughness of the alloy. and strength, while controlling the ratio of manganese to iron, optimizing the content of chromium and nickel to improve the plasticity and mechanical properties of the alloy.

Benefits of technology

It achieves mechanical properties similar to those of unadded recycled materials, while reducing the preparation cost, improving the toughness and strength of the alloy, and enhancing its recyclability, supporting the development of green closed-loop.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932205A_ABST
    Figure CN118932205A_ABST
Patent Text Reader

Abstract

The invention provides a heat-free aluminum alloy and a preparation method thereof. The preparation method comprises the steps that an aluminum alloy matrix raw material and a reclaimed material are sequentially subjected to the melting, alloying, refining and die casting processes, the heat-free aluminum alloy is obtained, the reclaimed material is an alloy containing the manganese element, and Fe forms a (FeMn) Al6 phase. Although the heat-free aluminum alloy prepared by the preparation method has higher iron element content, the heat-free aluminum alloy can obtain the same or closer mechanical properties such as toughness, strength and the like compared with an existing heat-free aluminum alloy product which is not added with a reclaimed material and is lower in iron element content, and the heat-free aluminum alloy also has lower preparation cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of automobile alloys, and in particular to a heat-free aluminum alloy and a preparation method thereof. Background Art

[0002] Aluminum alloy is an alloy obtained by adding a certain amount of other alloying elements to the metal aluminum as the matrix. It is one of the light metal materials. In addition to the general properties of aluminum, aluminum alloy also has some specific properties of the alloy due to the different types and quantities of alloying elements added. The density of aluminum alloy is 2.63~2.85g / cm 3 Its specific strength is close to that of high alloy steel, and its specific stiffness exceeds that of steel. It has good casting performance and plastic processing performance, good electrical and thermal conductivity, good corrosion resistance and weldability. It can be used as a structural material and is widely used in aerospace, aviation, transportation, construction, electromechanical, light chemical and daily necessities and other fields.

[0003] Aluminum alloy materials represented by A380 / 6061 have been widely used in the automotive industry, especially in new energy vehicle parts. This type of aluminum alloy is low-cost, can be produced on a large scale using recycled materials, and has high resource recycling. However, recycled aluminum contains high levels of impurity elements such as Fe, resulting in the material standard test bar performance only reaching a yield strength of 160MPa, a tensile strength of 320MPa, and an elongation of 3.5%, which cannot meet the use of new energy vehicle motor housings and other parts with higher strength requirements than castings.

[0004] In order to solve the above problems, the industry mostly uses low-Fe high-purity Al to produce high-strength and toughness die-cast aluminum alloys to ensure the mechanical properties of the alloy. This method has the following disadvantages: (1) The cost of aluminum alloys is high due to the high cost of raw materials, which hinders engineering applications; (2) Poor recyclability makes it difficult to achieve green closed-loop healthy development. In view of the existence of the above problems, the market urgently needs to study a low-cost and high-strength die-cast aluminum alloy to solve the pain points encountered by the automotive industry and the market. Summary of the invention

[0005] In view of the above-mentioned problems existing in the prior art, the present application provides a heat-free aluminum alloy and a preparation method thereof, so as to solve the problems of high cost and low strength of the existing recycled aluminum alloy materials.

[0006] The first aspect of the present application provides a method for preparing a heatless aluminum alloy, which comprises: subjecting an aluminum alloy matrix raw material and a recycled material to a melting, alloying, refining and die-casting process in sequence to obtain a heatless aluminum alloy, wherein the recycled material is an alloy containing manganese elements, so that at least part of the iron element in the heatless aluminum alloy forms a (FeMn)Al6 phase.

[0007] The second aspect of the present application also provides a heatless aluminum alloy, which includes the following composition, measured in percentage by weight: 7.0wt% to 12.0wt% Si, 0.4wt% to 2.0wt% Mg, 0.4wt% to 1.0wt% Mn, 0.1wt% to 0.5wt% Ti, 0.01wt% to 0.1wt% V, 1.0wt% to 5.0wt% Cu, 1.0wt% to 5.0wt% Zn, 0.01wt% to 0.1wt% La, 0.01wt% to 0.1wt% Ce, <0.5wt% Fe, <0.01wt% Pb, <0.01wt% Ca and the remainder Al, and part of the Fe forms a (FeMn)Al6 phase, or is prepared by the above-mentioned preparation method.

[0008] Beneficial effects:

[0009] Although the heatless aluminum alloy prepared by the above preparation method has a higher content of iron, it can obtain the same or similar mechanical properties such as toughness and strength as the existing heatless aluminum alloy products without added recycled materials and with lower iron content, and also has a lower preparation cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 This is the metallographic structure diagram of the aluminum alloy prepared in Example 3 of the present application. DETAILED DESCRIPTION

[0011] For simplicity, only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an unspecified range.

[0012] Unless otherwise specified, the terms used in this application have the well-known meanings commonly understood by those skilled in the art. Unless otherwise specified, the numerical values ​​of the parameters mentioned in this application can be measured by various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the embodiments of this application). It should be noted that, in the absence of conflict, the embodiments in this application and the features in the embodiments can be combined with each other.

[0013] The present application provides a method for preparing a heatless aluminum alloy, which comprises: subjecting an aluminum alloy matrix raw material and a recycled material to a melting, alloying, refining and die-casting process in sequence to obtain a heatless aluminum alloy, wherein the recycled material is an alloy containing manganese elements, so that at least part of the iron element in the heatless aluminum alloy forms a (FeMn)Al6 phase.

[0014] The term "aluminum alloy matrix raw material" in this application is defined in a broad sense as being capable of forming a high-strength and tough die-cast aluminum alloy (tensile strength R m ≥280MPa, yield strength R p0.2 ≥180MPa, elongation after fracture of 1.5% to 4.0%) can be used as the research object of this application. For example, the raw material of the aluminum alloy matrix is ​​a low-iron heatless aluminum alloy with an iron content of less than 0.15wt%. (FeMn)Al6 phase is Fe-Mn-Al phase.

[0015] The term "recycled material" in this application refers to aluminum alloys obtained by remelting and refining waste aluminum and aluminum alloy materials or aluminum-containing waste materials, and this application specifically selects aluminum alloys containing manganese. Such recycled materials usually have a high content of iron. Optionally, recycled materials include but are not limited to aluminum alloy A380 and / or aluminum alloy A6061.

[0016] Adding recycled materials to the aluminum alloy matrix raw material to prepare heat-free aluminum alloy can reduce its preparation cost on the one hand, and on the other hand, it can also enable the heat-free aluminum alloy prepared in this application to obtain the same or relatively close mechanical properties such as toughness and strength as the existing heat-free aluminum alloy products without adding recycled materials. Specifically, in the preparation method of heat-free aluminum, the use of recycled materials will introduce some impurity elements (such as Fe elements), and these elements (especially high content of Fe elements) will harm the strength and plasticity of the alloy. In order to solve the above problems, the present application introduces Mn elements by adding recycled materials containing manganese elements, so that it forms (FeMn)Al6 with impurity element Fe, and the plasticity of the obtained heat-free aluminum alloy can be effectively improved by modifying the needle-shaped Fe phase. In summary, although the heat-free aluminum alloy prepared by the above preparation method has a high content of iron, it can obtain the same or relatively close mechanical properties such as toughness and strength as the existing heat-free aluminum alloy products without adding recycled materials and with low iron content, and it also has a lower preparation cost.

[0017] The modified needle-like Fe phase refers to the needle-like shape before modification. The morphology after modification is as follows: Figure 1 shown.

[0018] By introducing manganese, the higher iron in the raw material can form (FeMn)Al6 phase, thereby reducing the adverse effects of excessive iron. In the mixture of aluminum alloy matrix raw material and recycled material, the weight ratio of manganese to iron can be adjusted according to the performance of the obtained heatless aluminum alloy, as long as it can be equivalent to or better than the performance of existing aluminum alloys, so there is no need for specific limitations. Exemplarily, in the mixture of aluminum alloy matrix raw material and recycled material, the weight ratio of manganese to iron is ≥1.5:1, and as the ratio increases, the performance will also improve accordingly. Optionally, the weight ratio of manganese to iron is 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2.0:1, 2.1:1, 2.2:1, 2.3:1, 2.4:1, 2.5:1, 2.6:1, 2.7:1, 2.8:1, 2.9:1, 3.0:1, 3.1 :1, 3.2:1, 3.3:1, 3.4:1, 3.5:1, 3.6:1, 3.7:1, 3.8:1, 3.9:1, 4.0:1, 4.1:1, 4.2:1, 4.4:1, 4.5:1, 4.6:1, 4.7:1, 4.8:1, 4.9:1, 5.0:1, 5.1:1, 5.2:1, 5.3:1, 5.4:1, 5.5:1, 5.6:1, 5.7:1, 5.8:1, or the range formed by any two of the above values. However, the manganese element cannot exceed a certain limit. Excessive manganese will also bring certain negative effects to the heat-free aluminum alloy, such as reduced hardness and shortened service life. Based on comprehensive consideration of cost and comprehensive performance, in a preferred embodiment, the weight ratio of manganese to iron in the mixture of aluminum alloy matrix raw material and recycled material is (2.25-4.2): 1. The weight ratio of manganese to iron in the mixture of aluminum alloy matrix raw material and recycled material includes but is not limited to the above range, and limiting it within the above range is conducive to making the obtained heatless aluminum alloy have relatively excellent hardness, service life and plasticity.

[0019] Recycled materials generally contain chromium and / or nickel, which are impurity elements for heatless aluminum alloys. If not treated, they may affect the performance of the heatless aluminum alloys.

[0020] In order to reduce or eliminate the influence of chromium on the plasticity of aluminum alloy elements, preferably, the content of chromium in the heatless aluminum alloy is ≤0.2wt%. Compared with other ranges, limiting the content of chromium within the above range can make Cr, Mn, Si, Fe and Al elements react at the same time to form (CrFeMnSi)Al6 phase, and transform the needle-shaped β(Fe2Si2Al9) phase into a short rod-shaped or nearly spherical structure, thereby further improving the plasticity index of the heatless aluminum alloy.

[0021] In order to weaken or eliminate the influence of nickel on the plasticity of aluminum alloy elements, preferably, in the heat-free aluminum alloy, the content of nickel is 0.01wt% to 0.2wt%. The content of nickel includes but is not limited to the above range, and limiting the content of nickel within this range is conducive to promoting the combination of Ni element, Fe element and Al element to form FeNiAl9 phase. The formation of this metal phase is conducive to improving the tensile strength and yield strength of the heat-free aluminum alloy, improving the high temperature strength and heat resistance, and preventing the alloy from deforming at high temperature, thereby having the advantages of being able to maintain the mechanical properties under low Fe element content under high Fe element content, reducing costs and strong recyclability. Optionally, the content of nickel in the heat-free aluminum alloy is 0.01wt%, 0.02wt%, 0.04wt%, 0.06wt%, 0.08wt%, 0.10wt%, 0.12wt%, 0.14wt%, 0.16wt%, 0.18wt%, 0.20wt%, or the range between any two of the above values. At the same time, when the heatless aluminum alloy contains both Ni and Cr, when the mass ratio of Ni to Cr is ≥1.5:1, the heatless aluminum alloy has more excellent mechanical properties and plasticity. Optionally, the mass ratio of Ni to Cr is 1.5:1, 1.8:1, 2.0:1, 2.3:1, 2.6:1, 2.9:1, 3.5:1, 4.0:1, 5.0:1, 6.0:1, 7.0:1, 8.0:1, 9.0:1, 10.0:1, or a range formed by any two of the above values.

[0022] In a preferred embodiment, during the die casting process, the temperature of the mold is 227°C to 230°C, the vacuum degree is 35mbar to 40mbar, and the casting temperature is 700°C to 710°C. The temperature, vacuum degree and casting temperature of the die casting process include but are not limited to the above ranges, and limiting them within the above ranges is beneficial to ensuring the uniformity and stability of the alloy composition on the one hand, and is also beneficial to reducing the probability of defects such as shrinkage cavities and pores on the other hand.

[0023] In a preferred embodiment, during the die casting process, when the injection position is less than 280 mm, the injection speed is 0.18 m / s to 0.22 m / s, and when the casting height is greater than 280 mm, the injection speed is 2.8 m / s to 3.5 m / s. Compared with other injection speeds, limiting it within the above range is conducive to further improving the uniformity and density of the internal metallographic structure of the formed alloy.

[0024] In a preferred embodiment, the pressure of the die-casting process is 67MPa-70MPa, and the temperature of the mold is 227°C-230°C. The pressure and mold temperature of the die-casting process include but are not limited to the above ranges. Limiting the pressure and mold temperature of the die-casting process to the above ranges can, on the one hand, make the molten liquid to be die-cast have better fluidity and reduce internal defects, and on the other hand, can also improve the density and strength of the heat-free aluminum alloy.

[0025] In a preferred embodiment, during the die-casting process, when demolding, the weight ratio of the release agent to the die-casting alloy is 1:(80-120).

[0026] The release agent can be selected from the commonly used types in the art, such as (German Geco) W8000.

[0027] In order to further improve the toughness, strength and elongation of the heat-free aluminum alloy, preferably, the aluminum alloy matrix raw material used in the present application has the following composition:

[0028] 7.0wt%~10.0wt% Si, 0.4wt%~1.2wt% Mg, 0.6wt%~0.8wt% Mn, 0.1wt%~0.2wt% Ti, 0.01wt%~0.03wt% V, 1.5wt%~4.0wt% Cu, 1.0wt%~4.0wt% Zn, 0.01wt%~0.1wt% La, 0.01wt%~0.1wt% Ce, <0.15wt% Fe, <0.01wt% Pb, <0.01wt% Ca and the balance Al.

[0029] The second aspect of the present application also provides a heatless aluminum alloy, which includes the following composition, measured in weight percentage: 7.0wt% to 12.0wt% Si, 0.4wt% to 2.0wt% Mg, 0.4wt% to 1.0wt% Mn, 0.1wt% to 0.5wt% Ti, 0.01wt% to 0.1wt% V, 1.0wt% to 5.0wt% Cu, 1.0wt% to 5.0wt% Zn, 0.01wt% to 0.1wt% La, 0.01wt% to 0.1wt% Ce, <0.5wt% Fe, <0.01wt% Pb, <0.01wt% Ca and the remainder Al, and at least part of the Fe forms a (FeMn)Al6 phase, or is obtained by using the above-mentioned method for preparing the heatless aluminum alloy.

[0030] Although the heatless aluminum alloy having the above composition or prepared by the above preparation method has a relatively high content of iron, it can obtain the same or similar mechanical properties such as toughness and strength as the existing heatless aluminum alloy products without added recycled materials and with a lower iron content, and also has a lower preparation cost.

[0031] In a preferred embodiment, the heatless aluminum alloy further includes ≤0.2wt% of Cr, measured by weight percentage. The heatless aluminum alloy may contain the Cr element or may not contain it. When the Cr element is included, at least part of the Cr forms a (CrFeMnSi)Al6 phase, which is beneficial to improve the plasticity of the heatless aluminum alloy. Optionally, the content of the Cr element in the heatless aluminum alloy is 0.01wt%, 0.02wt%, 0.04wt%, 0.06wt%, 0.08wt%, 0.10wt%, 0.12wt%, 0.14wt%, 0.16wt%, 0.18wt%, 0.19wt%, or a range between any two of the above values, measured by weight percentage.

[0032] In a preferred embodiment, the heatless aluminum alloy further comprises 0.01wt% to 0.2wt% Ni, at least part of which forms FeNiAl9 phase. Optionally, the content of Ni in the heatless aluminum alloy is 0.01wt%, 0.02wt%, 0.04wt%, 0.06wt%, 0.08wt%, 0.10wt%, 0.12wt%, 0.14wt%, 0.16wt%, 0.18wt%, 0.20wt%, or a range between any two of the above values.

[0033] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0034] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0035] The composition of the aluminum alloy matrix raw material used in the examples is shown in Table 1.

[0036] Table 1

[0037]

[0038]

[0039] The heat-free aluminum alloy in each embodiment is prepared by the following steps:

[0040] S1, mixing the aluminum alloy matrix raw material and the recycled material according to a predetermined ratio.

[0041] S2. The above raw materials are placed in a die-casting device for injection molding and die-casting in sequence to obtain sample 1. During the injection molding process, the casting temperature is 700°C~710°C, the mold temperature is 227°C~230°C, and the vacuum degree is 35mbar~40mbar; during the die-casting process, the casting pressure is 67MPa~70MPa; the release agent is W8000, and the weight ratio of the release agent to the die-casting alloy is 1:100.

[0042] S3, repeat steps S1-S2 to prepare samples 2 to 4.

[0043] S4, perform chemical composition test, mechanical property test and metallographic test on samples 1 to 4 respectively. Collect test data and average the results of chemical composition test and mechanical property test. The test samples are divided into heat treatment-free samples and heat treatment samples through mechanical property test.

[0044] The following methods are used during die casting and subsequent analysis:

[0045] GB / T 1196-2017 Aluminum ingots for remelting;

[0046] GB / T 7999 Photoelectric direct reading emission spectroscopy analysis method for aluminum and aluminum alloys;

[0047] HBZ 60-1996 X-ray photography inspection;

[0048] YS_T 492 Aluminum and aluminum alloy component additives;

[0049] GB / T 228.1-2021 Tensile test of metal materials;

[0050] GB / T 13822-2017 Die-casting nonferrous alloy specimens;

[0051] GB / T3246 Microstructure inspection method for deformed aluminum and aluminum alloy products.

[0052] The proportion of recycled material 1 added to each sample of Examples 1 to 4 is different. After adding recycled material 1, the composition of each element in the heatless aluminum alloy obtained is shown in Table 2. The percentage of recycled material added = weight of recycled material / (weight of recycled material+weight of aluminum alloy base material)*100%.

[0053] Table 2

[0054]

[0055] The above method was used to test its performance, and the test results are shown in Table 3.

[0056] Table 3

[0057]

[0058] In Table 3, R m Indicates tensile strength, R p0.2 It indicates the stress corresponding to the specified plastic elongation of 0.2%, A indicates the elongation after fracture, and the aging treatment is carried out in an oil bath at 200°C for 30 minutes.

[0059] F state (cast state) refers to the initial state of the alloy formed during the casting process, that is, the state of the metal structure and mechanical properties after solidification.

[0060] The metallographic structure of the aluminum alloy obtained in Example 3 is shown in Figure 1 .

[0061] The proportion of recycled material 2 added to each sample of Examples 5 to 8 is different. After adding recycled material 2, the composition of each element in the obtained heatless aluminum alloy is shown in Table 4.

[0062] Table 4

[0063]

[0064] The above method was used to perform performance test, and the test results are shown in Table 5.

[0065] Table 5

[0066]

[0067] The aging treatment in Table 5 is 30 min in an oil bath at 200°C.

[0068] The mechanical properties of existing low-Fe heat-treated aluminum alloys (iron content below 0.12wt%) are: m 280MPa~310MPa, R p0.2 170MPa~190MPa, elongation 2%~3%; in the aging state, R m 300MPa~330MPa, R p0.2 210MPa~240MPa, elongation at break 1.5%~3.0%.

[0069] As shown in Table 5, the heat-free aluminum alloys prepared in Examples 5 to 8 have high mechanical strength, toughness and elongation in both the cast state and the aged state, and are equivalent to or better than the performance of the existing low-Fe heat-treated aluminum alloys. In particular, when the added percentage of recycled material 2 is 35wt%, it can still maintain high performance. At the same time, when the heat-free aluminum alloy contains Ni and Cr elements at the same time, limiting the mass ratio of Ni element to Cr element within a certain range is conducive to improving the performance of the heat-free aluminum alloy.

[0070] Depend on Figure 1 It can be seen that the present application introduces the Mn element by adding recycled materials containing the manganese element, so that it can form (FeMn)Al6 (i.e., Fe-Mn-Al phase) with the impurity element Fe.

[0071] Although some exemplary embodiments of the present application have been illustrated and described, the present application is not limited to the disclosed embodiments. On the contrary, those skilled in the art will recognize that some modifications and changes may be made to the described embodiments without departing from the spirit and scope of the present application as described in the appended claims.

Claims

1. A method for preparing a heat-free aluminum alloy, characterized in that: The preparation method of the heat-free aluminum alloy comprises: subjecting an aluminum alloy matrix raw material and a recycled material to melting, alloying, refining and die-casting processes in sequence to obtain the heat-free aluminum alloy, wherein the recycled material is an alloy containing manganese elements, so that at least part of the iron element in the heat-free aluminum alloy forms a (FeMn)Al6 phase.

2. The method for preparing heatless aluminum alloy according to claim 1, characterized in that: In the mixture of the aluminum alloy matrix raw material and the recycled material, the weight ratio of manganese element to iron element is ≥1.5:1, preferably (1.5-5.8):1, and further preferably (2.25-4.2):

1.

3. The method for preparing heatless aluminum alloy according to claim 1 or 2, characterized in that: In the heatless aluminum alloy, the content of chromium element is ≤0.2wt%.

4. The method for preparing heatless aluminum alloy according to claim 1 or 2, characterized in that: In the heatless aluminum alloy, the content of nickel element is 0.01wt% to 0.2wt%.

5. The method for preparing a heatless aluminum alloy according to any one of claims 1 to 4, characterized in that: During the die-casting process, the temperature of the mold is 227° C. to 230° C., the vacuum degree is 35 mbar to 40 mbar, and the casting temperature is 700° C. to 710° C.

6. The method for preparing heatless aluminum alloy according to claim 5, characterized in that: In the die-casting process, when the injection position is less than 280 mm, the injection speed is 0.18 m / s to 0.22 m / s, and when the injection position is greater than 280 mm, the injection speed is 2.8 m / s to 3.5 m / s.

7. The method for preparing heatless aluminum alloy according to claim 1, characterized in that: The pressure of the die-casting process is 67MPa-70MPa, and the temperature of the mold is 227°C-230°C.

8. The method for preparing heatless aluminum alloy according to claim 1, characterized in that: During the die-casting process, when demolding, the weight ratio of the release agent to the die-casting alloy is 1:(80-120).

9. A heat-free aluminum alloy, characterized in that: Measured in percentage by weight, the heatless aluminum alloy comprises the following composition: 7.0wt% to 12.0wt% Si, 0.4wt% to 2.0wt% Mg, 0.4wt% to 1.0wt% Mn, 0.1wt% to 0.5wt% Ti, 0.01wt% to 0.1wt% V, 1.0wt% to 5.0wt% Cu, 1.0wt% to 5.0wt% Zn, 0.01wt% to 0.1wt% La, 0.01wt% to 0.1wt% Ce, <0.5wt% Fe, <0.01wt% Pb, <0.01wt% Ca and the remainder Al, and at least part of the Fe forms a (FeMn)Al6 phase, or is obtained by the preparation method of the heatless aluminum alloy described in any one of claims 1 to 8.

10. The heatless aluminum alloy according to claim 9, characterized in that: The heatless aluminum alloy further comprises ≤0.2wt% Cr by weight percentage, at least part of which forms a (CrFeMnSi)Al6 phase; and / or Calculated by weight percentage, the heatless aluminum alloy also includes 0.01wt% to 0.2wt% Ni, and at least part of the Ni forms a FeNiAl9 phase.

Citation Information

Cited By

  • Preparation method of regenerated high-strength heat-treatment-free die-casting aluminum alloy

    CN122189400A

  • Preparation method of recycled high-strength heat-free die-cast aluminum alloy

    CN122189400B