Ferrotitanium series hydrogen storage alloy easy to activate and preparation method thereof

By adding La and Zr to the ferrotitanium alloy and using specific process treatment, the problem of initial hydrogen absorption and activation of ferrotitanium alloy is solved, and efficient hydrogen absorption under mild conditions is achieved, which is suitable for hydrogen fuel cells and hydrogen storage.

CN118932213APending Publication Date: 2024-11-12XIAMEN SHENGYUAN GREEN ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410988552.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Iron titanium alloys are difficult to initially absorb and activate, require high temperature and hydrogen pressure conditions, and the activation process is complex, which affects its application efficiency.

Method used

By adding a very small amount of La and Zr to the titanium alloy and using specific smelting and in-situ heat treatment processes, the elemental composition of Ti1.09Zr0.01La0.01FexMny is formed, which improves the activation performance and hydrogen storage of the alloy and simplifies the activation process.

Benefits of technology

It significantly shortens the activation and incubation time of the alloy, improves the hydrogen storage amount and activation efficiency, and enables the alloy to absorb hydrogen directly under mild conditions, with a maximum hydrogen absorption of 1.76 wt% and above, suitable for hydrogen fuel cells and hydrogen storage. application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932213A_ABST
    Figure CN118932213A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of hydrogen storage alloys, in particular to an easily-activated ferrotitanium hydrogen storage alloy and a preparation method thereof. The element composition of the titanium-iron series hydrogen storage alloy easy to activate is Ti < 1.09 > Zr < 0.01 > La < 0.01 > Fe < x > Mn < y >, x and y respectively represent the atomic percentage of Fe and Mn, 0.8 < = x < 1.0, and 0.1 < = y < = 0.2. The hydrogen storage alloy provided by the invention is low in production cost, simple to prepare and easy to activate under mild conditions, and has a relatively good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrogen storage alloys, and in particular to an easily activated titanium-iron series hydrogen storage alloy and a preparation method thereof. Background Art

[0002] Titanium-iron alloy (TiFe alloy) is a hydrogen storage material with excellent performance and low cost, and is widely used in hydrogen storage, purification, hydrogen compressor and other fields. This alloy has the advantages of large hydrogen absorption and rapid hydrogen release, but it also faces some challenges in practical applications, especially the difficulty of initial hydrogen absorption and activation.

[0003] The difficulty in activating titanium-iron alloys is mainly reflected in the fact that they require high temperatures (about 250°C or above) and hydrogen pressure conditions for effective hydrogen absorption. In this case, the alloy needs to be activated through repeated hydrogen filling and evacuation operations so that it can effectively absorb and release hydrogen.

[0004] In order to improve the activation performance of titanium-iron alloys, researchers have conducted a series of explorations. These improvement methods include adjusting the relative content of alloying elements, improving processing technology, introducing suitable alloying elements (such as Mn, Co, etc.), and surface modification. For example, by excessively adding suitable Ti elements, transition metal elements or rare earth elements, the activation performance of TiFe alloys can be effectively improved. In addition, reducing the density of the alloy surface to promote the rapid entry of hydrogen atoms into the alloy surface, increasing the phase interface or introducing crystal defects to improve the diffusion capacity of hydrogen atoms are also effective strategies to improve its activation performance.

[0005] Therefore, it is necessary to provide an easily activated titanium-iron hydrogen storage alloy. Summary of the invention

[0006] In order to solve the problem of difficulty in initial hydrogen absorption and activation of titanium-iron alloy in the above-mentioned prior art, the present invention provides an easily activated titanium-iron hydrogen storage alloy and a preparation method thereof;

[0007] One of the purposes of the present invention is to provide an easily activated titanium-iron hydrogen storage alloy, wherein the element composition of the easily activated titanium-iron hydrogen storage alloy is Ti 1.09 Zr 0.01 La 0.01 Fe x Mn y ;

[0008] Wherein x and y represent the atomic percentages of Fe and Mn respectively, 0.8≤x<1.0, 0.1≤y≤0.2.

[0009] The present invention provides a titanium-iron hydrogen storage alloy, the titanium and iron elements used are low in cost and convenient for large-scale industrial application. The present invention has found through research that adding a very small amount of La (lanthanum) and Zr (zirconium) to a TiFe alloy containing Mn (manganese) can significantly improve the activation performance of the alloy, shorten the incubation time when the alloy is activated, and significantly improve the hydrogen storage capacity. This is because Zr and Mn can form a small amount of ZrMn2 intermetallic compounds, which can reasonably improve the activation performance of the alloy and increase the hydrogen storage capacity, but excessive Zr addition will lead to a decrease in the hydrogen storage capacity of the alloy, and adding a very small amount of La can appropriately refine the grains of the titanium-iron alloy, and grain refinement can not only improve the strength and toughness of the alloy, but also increase the specific surface area of ​​the alloy, provide more hydrogen storage sites, thereby increasing the hydrogen storage capacity, and, in particular, under the hydrogen storage alloy ratio provided by the present invention, if lanthanum is further added, the phase equilibrium and microstructure of the alloy will be destroyed, resulting in a decrease in hydrogen storage performance, and other unfavorable factors will also be introduced, such as increasing the brittleness of the alloy.

[0010] In the present invention, x=0.8-1.0, and the specific x can be 0.80, 0.81, 0.82, 0.83, 0.84, 0.85, 0.86, 0.87, 0.88, 0.89, 0.90, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99, 1.0, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0011] In the present invention, y=0.1-0.2, and y can specifically be 0.1, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.20, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0012] In one embodiment, the easily activated titanium-iron hydrogen storage alloy is Ti 1.09 La 0.01 Fe 0.89 Mn 0.17 Zr 0.01 、Ti 1.09 La 0.01 Fe 0.86 Mn 0.2 Zr 0.01 , or Ti 1.09 La 0.01 Fe 0.96 Mn 0.1 Zr 0.01 A combination of one or more of .

[0013] In one embodiment, the elemental composition of the easily activated titanium-iron hydrogen storage alloy is 0.8≤x≤0.9, 0.12≤y≤0.2. The present invention has found that when x=0.8-0.9, the incubation period of the first hydrogen absorption of the easily activated titanium-iron hydrogen storage alloy is significantly shorter; and when 0.8≤x≤0.9 and 0.12≤y≤0.2, the fluctuation of the maximum hydrogen storage capacity of the hydrogen storage alloy at different temperatures is significantly reduced.

[0014] In the hydrogen storage alloy ratio provided by the present invention, the appropriate addition of Fe element can promote the phase change and crystal structure adjustment of the alloy during the activation process, thereby shortening the activation time and improving the activation efficiency. However, increasing the content of Fe element is likely to increase the thermal expansion coefficient of the alloy, making it prone to thermal deformation in a high temperature environment, thereby affecting the activation performance; while the control of the Mn element content can promote the surface reconstruction and hydrogen diffusion process of the alloy during the activation process, thereby accelerating the activation reaction. However, in the hydrogen storage alloy ratio provided by the present invention, when the content of Mn element is reduced, the stability of the hydride decreases. As the temperature increases, the decomposition of the hydride is too fast, which in turn reduces the hydrogen storage capacity, causing the hydrogen storage capacity of the alloy to fluctuate significantly.

[0015] The second object of the present invention is to provide a method for preparing the easily activated titanium-iron hydrogen storage alloy described in the first object, the preparation method comprising the following steps:

[0016] (1) weighing elemental metals according to atomic ratio and mixing them to obtain a mixed material;

[0017] (2) smelting the mixed material obtained in step (1) to obtain a cast alloy;

[0018] (3) subjecting the cast alloy obtained in step (2) to in-situ heat treatment and cooling to obtain a hydrogen storage alloy ingot.

[0019] The preparation method described in the present invention is based on a specific atomic ratio for formulation. The easily activated ferro-titanium hydrogen storage alloy can be obtained through smelting and in-situ heat treatment, which effectively solves the problem of difficulty in initial hydrogen absorption and activation of ferro-titanium hydrogen storage alloys. The method is simple, fast and effective, and is easy to promote and use on a large scale. It has broad application prospects in the fields of nickel-hydrogen batteries, hydrogen fuel cell hydrogen sources, hydrogen storage and transportation.

[0020] In one embodiment, the purity of the elemental metal in step (1) is ≥99.5wt%, and the elemental metal includes titanium, lanthanum, zirconium, iron and manganese.

[0021] The smelting in step (2) of the present invention is carried out under the protection of a protective gas, which can be a gas that does not react with the raw materials, such as nitrogen or an inert gas. After smelting, the alloy is allowed to cool to room temperature along with the copper crucible, which is then turned over and smelted again.

[0022] In one embodiment, the smelting in step (2) is performed in a vacuum induction suspension furnace.

[0023] In one embodiment, the smelting power in step (2) is 50-130 kW, and the power can specifically be 50 kW, 60 kW, 70 kW, 80 kW, 90 kW, 100 kW, 110 kW, 120 kW, 130 kW, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0024] Preferably, the smelting in step (2) includes a first smelting power and a second smelting power, and the first smelting power is lower than the second smelting power;

[0025] Preferably, the smelting in step (2) includes continuously smelting at a first smelting power until the mixed material begins to melt, and then increasing the smelting power until the raw material is completely melted, and the smelting power when the raw material is completely melted is a second smelting power;

[0026] Preferably, in step (2), the first smelting power is increased to the second smelting power in a step-by-step manner;

[0027] Preferably, the gradient of the step-by-step increase is 10-20 kW, which may be 10 kW, 15 kW, 20 kW, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable;

[0028] Preferably, the first smelting power is 50 kW, and the second smelting power is 130 kW.

[0029] In one embodiment, the smelting in step (2) is performed 3 to 5 times, and the smelting may be performed 3, 4 or 5 times.

[0030] Preferably, the smelting in step (2) is performed three times;

[0031] Preferably, the smelting time in step (2) is 120 to 300 seconds, and the smelting time can specifically be 120 seconds, 130 seconds, 140 seconds, 150 seconds, 200 seconds, 250 seconds, 300 seconds, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0032] Preferably, after the smelting in step (2) is completed, 90 to 150 seconds, the in-situ heat treatment is performed at a power lower than the power at which the alloy begins to melt during the smelting. Preferably, after the smelting in step (2) is completed, the in-situ heat treatment is performed at a power lower than the power at which the alloy begins to melt during the smelting.

[0033] It should be noted that in the present invention, in-situ heat treatment is performed to improve the microstructure and performance of the alloy. Controlling the in-situ heat treatment at a power lower than the power at which the alloy begins to melt during smelting can effectively avoid unnecessary diffusion and segregation caused by overheating of the alloy and cracks on the alloy surface.

[0034] Preferably, the vacuum degree of the smelting in step (2) is ≤5.0×10 -3 Pa.

[0035] In one embodiment, the power of the in-situ heat treatment in step (3) is 20-35 kW, and the power can specifically be 20 kW, 21 kW, 22 kW, 23 kW, 24 kW, 25 kW, 30 kW, 35 kW, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0036] Preferably, the time of the in-situ heat treatment is 5 to 10 minutes, and the time may be 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0037] Preferably, the in-situ heat treatment time is 5 minutes.

[0038] It is worth noting that the in-situ heat treatment technology used in the alloy preparation process can change the microstructural characteristics of the material, such as grain size, phase composition and distribution; at the same time, the in-situ heat treatment technology avoids the process of removing the alloy ingot by directly heating or cooling the alloy ingot at the location of the ingot, thereby simplifying the process flow, reducing the process time, and making the entire processing process faster and improving production efficiency; since the alloy ingot is in its original fixed position during the in-situ heat treatment, the deformation and residual stress caused by movement or repositioning are reduced.

[0039] In one embodiment, the cooling in step (3) further includes a crushing process;

[0040] Preferably, the average particle size of the easily activated titanium-iron hydrogen storage alloy obtained after crushing is 40 to 100 meshes, and the average particle size can be 40 meshes, 50 meshes, 60 meshes, 70 meshes, 80 meshes, 90 meshes, 100 meshes, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0041] Preferably, the surface layer of the alloy ingot is cut off before the crushing to remove the surface oxide layer, which is beneficial to the subsequent activation performance test;

[0042] Preferably, the thickness of the surface layer is 1 to 2 mm;

[0043] Preferably, the cooling time is 20 minutes.

[0044] Based on the above, compared with the prior art, the easily activated titanium-iron hydrogen storage alloy provided by the present invention has at least one of the following beneficial technical effects:

[0045] The titanium-iron series hydrogen storage alloy provided by the present invention has good activation performance, a simple activation process, high safety, and can directly absorb hydrogen under relatively mild conditions. The maximum hydrogen absorption capacity of the alloy at room temperature reaches 1.76wt% or more.

[0046] Other features and beneficial effects of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other beneficial effects of the present invention can be realized and obtained by the structures particularly pointed out in the description, claims and drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0048] Figure 1 Ti prepared in Example 1 1.09 La 0.01 Fe 0.89 Mn 0.17 Zr 0.01 Activation curves of hydrogen storage alloys;

[0049] Figure 2 The Ti prepared in Example 1 1.09 La 0.01 Fe 0.89 Mn 0.17 Zr 0.01 PCT curves of hydrogen absorption and desorption of hydrogen storage alloys at 303K, 323K and 333K respectively;

[0050] Figure 3 Ti prepared in Example 2 1.09 La 0.01 Fe 0.86 Mn 0.2 Zr 0.01 Activation curves of hydrogen storage alloys;

[0051] Figure 4 Ti prepared in Example 2 1.09 La 0.01 Fe 0.86 Mn0.2 Zr 0.01 PCT curves of hydrogen absorption and desorption of hydrogen storage alloys at 303K, 323K and 333K respectively;

[0052] Figure 5 Ti prepared in Example 3 1.09 La 0.01 Fe 0.96 Mn 0.1 Zr 0.01 Activation curves of hydrogen storage alloys;

[0053] Figure 6 Ti prepared in Example 3 1.09 La 0.01 Fe 0.96 Mn 0.1 Zr 0.01 PCT curves of hydrogen absorption and desorption of hydrogen storage alloys at 303K, 323K and 333K;

[0054] Figure 7 XRD diffraction spectra of hydrogen storage alloys of Examples 1-3;

[0055] Figure 8 Ti prepared in Comparative Example 1 1.04 La 0.06 Fe 0.86 Mn 0.1 Zr 0.04 Activation curves of hydrogen storage alloys;

[0056] Fig. 9 Ti prepared in Comparative Example 1 1.04 La 0.06 Fe 0.86 Mn 0.1 Zr 0.04 PCT curve of hydrogen absorption and desorption of hydrogen storage alloy at 303K;

[0057] Fig.10 Ti prepared in Comparative Example 2 1.09 La 0.01 Fe 0.86 Mn 0.1 Zr 0.04 Activation curves of hydrogen storage alloys;

[0058] Fig.11 Ti prepared in Comparative Example 2 1.09 La 0.01 Fe 0.86 Mn 0.1 Zr 0.04 PCT curves of hydrogen absorption and desorption of hydrogen storage alloy at 303K. DETAILED DESCRIPTION

[0059] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments; the technical features designed in different implementation modes of the present invention described below can be combined with each other as long as they do not conflict with each other; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0060] Example 1

[0061] The hydrogen storage alloy Ti of this embodiment 1.09 La 0.01 Fe 0.89 Mn 0.17 Zr 0.01 150g of raw materials are weighed according to the alloy proportion, and the purity of the metal element used in the experiment is above 99.5%. The preparation method of the hydrogen storage alloy is as follows:

[0062] The ingredients are placed into the crucible of the vacuum induction suspension furnace according to their melting points, and then vacuumed to 5×10 -3 After the pressure drops below Pa, argon is filled in to clean the furnace. Repeat the above cleaning process twice, and then melt in a high-purity argon atmosphere. First melt at a power of 50kW, the raw materials begin to melt, and slowly increase the power until the power increases to 130kW, the raw materials are completely melted, and an alloy ingot is formed after cooling for 20 minutes. Take it out and turn it over and put it into the crucible for further melting. The above cleaning process is also carried out. After repeating the melting three times, in-situ heat treatment is performed for 5 minutes to ensure uniform alloy composition. Use a precision cutting machine to cut off the surface of the alloy ingot, and then mechanically crush the alloy ingot for hydrogen storage performance testing.

[0063] The above Ti 1.09 La 0.01 Fe 0.89 Mn 0.17 Zr 0.01 The activation test conditions of hydrogen storage alloy are as follows:

[0064] Take 1.59g alloy powder and put it into the sample chamber of the PCT tester. First, evacuate it at 353K for 1h and then fill it with 5MPa hydrogen to absorb hydrogen. Then, evacuate it at 303K for 1h and then fill it with 5MPa hydrogen to absorb hydrogen. Cycle twice under this condition until the alloy reaches the maximum hydrogen absorption and activation is completed. Figure 1 As shown, the hydrogen storage alloy can absorb hydrogen quickly for the first time at 353K, and can absorb hydrogen quickly and reach the maximum amount of hydrogen absorption in the second time. The maximum amount of hydrogen absorbed by the hydrogen storage alloy at 303K is 1.71wt%.

[0065] The above Ti 1.09 La 0.01 Fe 0.89 Mn 0.17 Zr 0.01 The PCT test conditions for hydrogen storage alloy absorption and desorption are as follows:

[0066] The test temperatures were 303K, 323K and 333K respectively, and the hydrogen pressure was 5MPa. Figure 2 The PCT curves of hydrogen absorption and desorption show that the maximum hydrogen storage capacity of the hydrogen storage alloy at 303K, 323K and 333K are 1.76wt%, 1.72wt% and 1.66wt%, respectively.

[0067] The Ti obtained in this example 1.09 La 0.01 Fe 0.89 Mn 0.17 Zr 0.01 The XRD diffraction pattern is as follows Figure 7 As shown, the diffraction peak of TiFe was observed, and no new substance was generated.

[0068] Example 2

[0069] The hydrogen storage alloy Ti of this embodiment 1.09 La 0.01 Fe 0.86 Mn 0.2 Zr 0.01 150g of raw materials are weighed according to the alloy proportion, and the purity of the metal element used in the experiment is above 99.5%. The preparation method of the hydrogen storage alloy is as follows:

[0070] The ingredients are placed into the crucible of the vacuum induction suspension furnace according to their melting points, and then vacuumed to 5×10 -3 After the pressure drops below Pa, argon is filled in to clean the furnace. Repeat the above cleaning process twice, and then melt in a high-purity argon atmosphere. First melt at a power of 50kW, the raw materials begin to melt, and slowly increase the power until the power increases to 130kW, the raw materials are completely melted, and an alloy ingot is formed after cooling for 20 minutes. Take it out and turn it over and put it into the crucible for further melting. The above cleaning process is also carried out. After repeating the melting three times, in-situ heat treatment is performed for 5 minutes to ensure uniform alloy composition. Use a precision cutting machine to cut off the surface of the alloy ingot, and then mechanically crush the alloy ingot for hydrogen storage performance testing.

[0071] The above Ti 1.09 La 0.01 Fe 0.86 Mn 0.2 Zr 0.01 The activation test conditions of hydrogen storage alloy are as follows:

[0072] Take 1.56g alloy powder and put it into the sample chamber of the PCT tester. Pre-evacuate at 353K for 1h and then fill it with 5MPa hydrogen to absorb hydrogen. Then evacuate at 303K for 1h and fill it with 5MPa hydrogen to absorb hydrogen. Cycle twice under this condition until the alloy reaches the maximum hydrogen absorption and activation is completed. Figure 3 As shown, the hydrogen storage alloy can absorb hydrogen quickly for the first time at 353K, and can absorb hydrogen quickly and reach the maximum amount of hydrogen absorption in the second time. The maximum amount of hydrogen absorbed by the hydrogen storage alloy at 303K is 1.69wt.%.

[0073] The above Ti 1.09 La 0.01 Fe 0.86 Mn 0.2 Zr 0.01 The PCT test conditions for hydrogen storage alloy absorption and desorption are as follows:

[0074] The test temperatures were 303K, 323K and 333K respectively, and the hydrogen pressure was 5MPa. Figure 4 The PCT curves of hydrogen absorption and desorption show that the maximum hydrogen storage capacity of the hydrogen storage alloy at 303K, 323K and 333K are 1.74wt%, 1.73wt% and 1.70wt%, respectively.

[0075] The Ti obtained in this example 1.09 La 0.01 Fe 0.86 Mn 0.2 Zr 0.01 The XRD diffraction pattern is as follows Figure 7 As shown, the diffraction peak of TiFe was observed, and no new substance was generated.

[0076] Example 3

[0077] The hydrogen storage alloy Ti of this embodiment 1.09 La 0.01 Fe 0.96 Mn 0.1 Zr 0.01 150g of raw materials are weighed according to the alloy proportion, and the purity of the metal element used in the experiment is above 99.5%. The preparation method of the hydrogen storage alloy is as follows:

[0078] The ingredients are placed into the crucible of the vacuum induction suspension furnace according to their melting points, and then vacuumed to 5×10 -3After the pressure drops below Pa, argon is filled in to clean the furnace. Repeat the above cleaning process twice, and then melt in a high-purity argon atmosphere. First melt at a power of 50kW, the raw materials begin to melt, and slowly increase the power until the power increases to 130kW, the raw materials are completely melted, and an alloy ingot is formed after cooling for 20 minutes. Take it out and turn it over and put it into the crucible for further melting. The above cleaning process is also carried out. After repeating the melting three times, in-situ heat treatment is performed for 5 minutes to ensure uniform alloy composition. Use a precision cutting machine to cut off the surface of the alloy ingot, and then mechanically crush the alloy ingot for hydrogen storage performance testing.

[0079] The above Ti 1.09 La 0.01 Fe 0.96 Mn 0.1 Zr 0.01 The activation test conditions of hydrogen storage alloy are as follows:

[0080] Take 1.61g alloy powder and put it into the sample chamber of the PCT tester. Pre-evacuate at 353K for 1h and then fill it with 5MPa hydrogen to absorb hydrogen. Then evacuate at 303K for 1h and fill it with 5MPa hydrogen to absorb hydrogen. Cycle twice under this condition until the alloy reaches the maximum hydrogen absorption and activation is completed. Figure 5 As shown in the figure, the hydrogen storage alloy absorbs hydrogen slowly for the first time at 353K, but can absorb hydrogen quickly and reach the maximum amount of hydrogen absorption in the second time. The maximum amount of hydrogen absorbed by the hydrogen storage alloy at 303K can reach 1.70wt%.

[0081] The above Ti 1.09 La 0.01 Fe 0.96 Mn 0.1 Zr 0.01 The PCT test conditions for hydrogen storage alloy absorption and desorption are as follows:

[0082] The test temperatures were 303K, 323K and 333K respectively, and the hydrogen pressure was 5MPa. Figure 6 The PCT curves of hydrogen absorption and desorption show that the maximum hydrogen storage capacity of the hydrogen storage alloy at 303K, 323K and 333K are 1.71wt%, 1.59wt% and 1.48wt%, respectively.

[0083] The Ti obtained in this example 1.09 La 0.01 Fe 0.96 Mn 0.1 Zr 0.01 The XRD diffraction pattern is as follows Figure 7 As shown, the diffraction peak of TiFe was observed, and no new substance was generated.

[0084] Comprehensive analysis of Examples 1-3 shows that the hydrogen storage alloy provided by the present invention has excellent easy activation performance, short activation incubation time and high hydrogen storage capacity;

[0085] From the comparative analysis of Examples 1-3, it can be seen that in the hydrogen storage alloy provided by the present invention, when the atomic percentage x of Fe is greater than 0.9 and the atomic percentage y of Mn is less than 0.12, its maximum hydrogen storage capacity at different temperatures has significant fluctuations, while when x is between 0.8 and 0.9 and y is between 0.12 and 0.2, the fluctuation of its maximum hydrogen storage capacity at different temperatures is significantly reduced.

[0086] Comparative Example 1

[0087] The hydrogen storage alloy Ti of this comparative example 1.04 La 0.06 Fe 0.86 Mn 0.1 Zr 0.04 Weigh 150 g of raw materials according to the alloy proportion, place them in a copper crucible of an induction suspension furnace, and evacuate to 5 × 10 -3 Pa, under the protection of argon atmosphere, adjust the power to heat the alloy, and when the alloy is completely melted, perform in-situ heat treatment for 5 minutes, and cool it to room temperature to obtain an alloy ingot. Then crush the alloy, load the alloy powder into the sample chamber of the PCT tester, evacuate it at 353K for 1 hour in advance, and then fill it with 5MPa hydrogen for hydrogen absorption. Cycle twice under this condition, then evacuate it at 303K for 1 hour and fill it with 5MPa hydrogen for hydrogen absorption, until the alloy reaches the maximum hydrogen absorption and activation is completed. At the same time, PCT test is carried out under the conditions of 303K and hydrogen pressure of 5MPa.

[0088] The test results of the alloy prepared in Comparative Example 1 are as follows: Figure 8 and 9 As shown in the figure, it can be seen from the comparison of the results that although higher La and Zr contents can make the alloy have better activation performance under milder conditions, the maximum hydrogen storage capacity at room temperature can only reach 1.61wt%.

[0089] Comparative Example 2

[0090] The hydrogen storage alloy Ti of this comparative example 1.09 La 0.01 Fe 0.86 Mn 0.1 Zr 0.04 Weigh 150 g of raw materials according to the alloy proportion, place them in a copper crucible of an induction suspension furnace, and evacuate to 5 × 10 -3Pa, under the protection of argon atmosphere, adjust the power to heat the alloy, and when the alloy is completely melted, perform in-situ heat treatment for 5 minutes, and cool it to room temperature to obtain an alloy ingot. Then crush the alloy, load the alloy powder into the sample chamber of the PCT tester, evacuate it at 353K for 1 hour in advance, and then fill it with 5MPa hydrogen for hydrogen absorption. Cycle twice under this condition, then evacuate it at 303K for 1 hour and fill it with 5MPa hydrogen for hydrogen absorption, until the alloy reaches the maximum hydrogen absorption and activation is completed. At the same time, PCT test is carried out under the conditions of 303K and hydrogen pressure of 5MPa.

[0091] The test results of the alloy prepared in Comparative Example 2 are as follows: Fig.10 and 11 As shown, from the comparison of the results, it can be seen that by keeping the Zr content at a higher level and reducing the La content, the hydrogen storage capacity of the alloy does not show an increasing trend, but rather decreases slightly, and the maximum hydrogen storage capacity is 1.57wt%.

[0092] Comparative Example 3

[0093] The hydrogen storage alloy Ti of this comparative example 1.09 La 0.01 FeMn 0.1 Zr 0.01 Weigh 150 g of raw materials according to the alloy proportion, place them in a copper crucible of an induction suspension furnace, and evacuate to 5 × 10 -3 Pa, under the protection of argon atmosphere, adjust the power to heat the alloy, and when the alloy is completely melted, perform in-situ heat treatment for 5 minutes, and cool it to room temperature to obtain an alloy ingot. Then the alloy is crushed, and the alloy powder is loaded into the sample chamber of the PCT tester, which is pre-evacuated at 353K for 1h and then filled with 5MPa hydrogen for hydrogen absorption. It is cycled twice under this condition and it is found that it is difficult to activate at 353K.

[0094] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. An easily activated titanium-iron hydrogen storage alloy, characterized in that: The element composition of the easily activated titanium-iron hydrogen storage alloy is Ti 1.09 Zr 0.01 La 0.01 Fe x Mn y ; Wherein x and y represent the atomic percentages of Fe and Mn respectively, 0.8≤x<1.0, 0.1≤y≤0.

2.

2. The easily activated titanium-iron hydrogen storage alloy according to claim 1, characterized in that: The easily activated titanium-iron hydrogen storage alloy is Ti 1.09 La 0.01 Fe 0.89 Mn 0.17 Zr 0.01 、Ti 1.09 La 0.01 Fe 0.86 Mn 0.2 Zr 0.01 , or Ti 1.09 La 0.01 Fe 0.96 Mn 0.1 Zr 0.01 A combination of one or more of .

3. The easily activated titanium-iron hydrogen storage alloy according to claim 1, characterized in that: The element composition of the easily activated titanium-iron hydrogen storage alloy is 0.8≤x≤0.9, and 0.12≤y≤0.

2.

4. A method for preparing an easily activated titanium-iron hydrogen storage alloy as claimed in any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: (1) weighing elemental metals according to atomic ratio and mixing them to obtain a mixed material; (2) smelting the mixed material obtained in step (1) to obtain a cast alloy; (3) subjecting the cast alloy obtained in step (2) to in-situ heat treatment and cooling to obtain a hydrogen storage alloy ingot.

5. The preparation method according to claim 4, characterized in that: The purity of the elemental metal in step (1) is ≥99.5wt%.

6. The preparation method according to claim 4, characterized in that: The smelting in step (2) is carried out in a vacuum induction suspension furnace.

7. The preparation method according to claim 4, characterized in that: The smelting power in step (2) is 50-130 kW; Preferably, the smelting in step (2) includes a first smelting power and a second smelting power, and the first smelting power is lower than the second smelting power; Preferably, the smelting in step (2) includes continuously smelting at a first smelting power until the mixed material begins to melt, and then increasing the smelting power until the raw material is completely melted, and the smelting power when the raw material is completely melted is a second smelting power; Preferably, in step (2), the first smelting power is increased to the second smelting power in a step-by-step manner; Preferably, the gradient of the step-by-step boost is 10-20kW; Preferably, the first smelting power is 50 kW, and the second smelting power is 130 kW.

8. The preparation method according to claim 4, characterized in that: The smelting in step (2) is repeated 3 to 5 times; Preferably, the smelting in step (2) is performed three times; Preferably, the smelting time in step (2) is 120 to 300 seconds; Preferably, 90 to 150 seconds after the smelting in step (2) is completed, an in-situ heat treatment is performed at a power lower than the power at which the alloy begins to melt during the smelting; Preferably, the vacuum degree of the smelting in step (2) is ≤5.0×10 -3 Pa.

9. The preparation method according to claim 4, characterized in that: The power of the in-situ heat treatment in step (3) is 20 to 35 kW; Preferably, the in-situ heat treatment time is 5 to 10 minutes; Preferably, the in-situ heat treatment time is 5 minutes.

10. The preparation method according to claim 4, characterized in that: Step (3) further comprises a crushing process after cooling; Preferably, the average particle size of the easily activated titanium-iron hydrogen storage alloy obtained after crushing is 40 to 100 meshes; Preferably, the surface layer of the alloy ingot is cut off before the crushing; Preferably, the thickness of the surface layer is 1 to 2 mm; Preferably, the cooling time is 20 minutes.