Al-Mn alloy and preparation method thereof

By adding silicon and copper to Al-Mn alloy and adopting a specific process flow, the problem of insufficient performance of Al-Mn alloy is solved, and the high tensile strength, yield strength and elongation are improved, satisfying customers' high Performance product requirements.

CN118932221APending Publication Date: 2024-11-12JIANGSU ASIA PACIFIC LIGHT ALLOY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411021247.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing Al-Mn alloys cannot meet the customer's high requirements for tensile strength ≥160MPa, yield strength ≥80MPa and elongation ≥20%, limiting their application range.

Method used

By appropriate addition of silicon and copper to the Al-Mn alloy and using specific melting, refining, casting and extrusion processes, including high-purity argon refining, double-layer filtration and vacuum direct-cooling casting, combining gradient preheating and low temperature Fast continuous extrusion to improve the thermal processing and forging performance of the alloy.

Benefits of technology

It significantly improves the tensile strength, yield strength and elongation of Al-Mn alloy, meets customers' requirements for high-performance products, and improves its thermodynamic performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of wrought aluminum alloy material preparation, and particularly relates to an Al-Mn alloy and a preparation method thereof. The Al-Mn alloy comprises, by mass, 0.45%-0.6% of Si, smaller than or equal to 0.3% of Fe, 0.45%-0.55% of Cu, 1.25%-1.35% of Mn, smaller than or equal to 0.05% of Mg, smaller than or equal to 0.1% of Zn, smaller than or equal to 0.05% of Ti, smaller than or equal to 0.05% of Cr, smaller than or equal to 0.05% of the single content of other impurities, smaller than or equal to 0.15% of the total amount of the impurities and the balance Al. On the basis of an aluminum-manganese alloy, silicon and copper are properly added, the advantage of corrosion resistance of the Al-Mn alloy is reserved, the forging performance of the Al-Mn alloy during hot working is remarkably improved, the heat treatment strengthening effect is improved, and subsequent machining treatment is facilitated. The aluminum alloy product has high strength, and when an extruded product is in an extruded state, the tensile strength is larger than or equal to 160 MPa, the yield strength is larger than or equal to 80 MPa, and the ductility is larger than or equal to 20%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of deformed aluminum alloy material preparation, and specifically relates to an Al-Mn alloy and a preparation method thereof. Background Art

[0002] With the rapid development of my country's new energy vehicle industry, the use of aluminum alloy materials in automobiles has become more mature. Due to the good corrosion resistance, welding performance and processing performance of Al-Mn alloy, the use of Al-Mn alloy is also gradually increasing, but due to the limitations of its strength and heat treatment capacity, the application range of Al-Mn alloy is not as wide as other types of aluminum alloys. Some customers need a product with good plasticity and certain forging performance. The customer's requirements for Al-Mn alloy are to meet the following conditions at the same time: tensile strength ≥160MPa, yield strength ≥80MPa, elongation ≥20%. The existing Al-Mn alloy cannot meet the above requirements. Summary of the invention

[0003] The purpose of the present invention is to overcome the deficiencies in the prior art and provide an Al-Mn alloy and a preparation method thereof. The present invention improves the competitiveness of Al-Mn alloy products by improving the strength problem of the Al-Mn alloy itself, and the obtained Al-Mn alloy has the characteristics of high performance and high forging performance, which can meet the subsequent processing of its customers and the system function requirements they need to achieve.

[0004] In order to achieve the above technical objectives, the technical solution adopted by the embodiment of the present invention is:

[0005] In a first aspect, an embodiment of the present invention provides an Al-Mn alloy, comprising the following components, by mass percentage: Si 0.45%-0.6%, Fe≤0.3%, Cu 0.45%-0.55%, Mn 1.25%-1.35%, Mg≤0.05%, Zn≤0.1%, Ti≤0.05%, Cr≤0.05%, the individual content of other impurities ≤0.05%, the total amount of impurities ≤0.15%, and the balance is Al.

[0006] In a second aspect, an embodiment of the present invention provides a method for preparing the Al-Mn alloy according to the first aspect, comprising the following steps:

[0007] (1) Melting: The raw material is aluminum ingots of grade AL99.70 in GB / T 1196-2008 standard, which are put into the furnace and heated to 730-760°C for melting;

[0008] (2) Slag removal: When the temperature is 730-760℃, sprinkle the slag remover evenly into the furnace and stir it thoroughly for 5-10 minutes. Use a rake to remove the slag on the surface of the aluminum liquid.

[0009] (3) Alloy: Add silicon, manganese and copper when the melt temperature is 730-760°C. After adding the alloy, stir for 10-15 minutes to evenly mix the components in the melt.

[0010] (4) Refining: When the melt temperature is 750-790°C, argon gas refining is used for 30-35 minutes. After refining, the scum on the liquid surface is scraped off.

[0011] (4) Standing: After refining, the melt is allowed to stand for 20-30 minutes;

[0012] (5) Casting: When the melt temperature is 770-790°C, the melt is cast into an ingot for standby use;

[0013] (6) Homogenization: The ingot obtained above is heated to 600±10° C., kept at this temperature for 5-5.2 hours, and rapidly cooled to obtain a homogenized ingot;

[0014] (7) Extrusion: The short aluminum alloy round cast rod is heated and then rapidly and continuously extruded at low temperature to obtain an aluminum alloy extruded tube billet.

[0015] Furthermore, the amount of slag remover added in step (2) is 0.5 kg / ton of aluminum.

[0016] Furthermore, during refining in step (4), argon gas with a purity of more than 99.7% is introduced; the refining agent used during refining is a fluorine-free and sodium-free granular refining agent, and the amount used is 1-1.5 kg / ton of aluminum.

[0017] Furthermore, in step (5), during the casting process, Al5Ti1B aluminum titanium boron wire is added to refine the grains of the ingot, and the addition rate is 75-85cm / min. Online degassing is performed on the casting launder, and high-purity argon gas is introduced during degassing, with the argon content being more than 99.7%. Then, double-layer filtration is used to further purify the melt, and a vacuum direct cooling casting system is used for casting, with a casting rate of 115±5mm / min, to finally obtain an ingot.

[0018] Furthermore, the specific steps of extrusion in step (7) are: obtaining short-stock aluminum alloy round cast rods and molds → preheating the short-stock aluminum alloy round cast rods, mold barrels and molds → installing extrusion molds → loading short-stock aluminum alloy round cast rods → low-temperature rapid and continuous extrusion → water cooling to obtain aluminum alloy extruded long material profiles.

[0019] Furthermore, the short-stock aluminum alloy round cast rod adopts a gradient preheating method: the preheating temperature of the cast rod at the advanced die barrel end is high, and the preheating temperature at the backward die barrel end is low. The preheating temperature of the head of the short-stock aluminum alloy round cast rod is 460-480°C, and the decreasing gradient is 3-5°C / 100mm;

[0020] The preheating temperature of the mold barrel is 420-440°C;

[0021] The preheating temperature of the mold is 470-490°C.

[0022] Furthermore, the continuous extrusion conditions are as follows: the extrusion speed of the ejector pin is 1.2-1.8 mm / s, and the extrusion temperature is 20-440°C.

[0023] The technical solution provided by the embodiment of the present invention has the following beneficial effects:

[0024] The present invention appropriately adds silicon and copper on the basis of aluminum-manganese alloy, not only retains the corrosion resistance of Al-Mn alloy, but also significantly improves the forging performance of Al-Mn alloy during hot working, increases the heat treatment strengthening effect, and is beneficial to subsequent processing. The aluminum alloy product of the present invention has high strength, wherein when the extruded product is in an extruded state, the tensile strength is ≥160MPa, the yield strength is ≥80MPa, and the elongation is ≥20%. Compared with other aluminum alloys with similar properties, the alloy of the present invention has higher thermodynamic properties and good forging properties. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0026] Example 1

[0027] An Al-Mn alloy comprises the following components by mass percentage: Si 0.45%, Fe 0.05%, Cu 0.45%, Mn 1.25%, Mg 0.01%, Zn 0.01%, Ti 0.01%, Cr 0.01%, other impurities each having a content of ≤0.05%, a total amount of impurities of ≤0.15%, and the balance being Al.

[0028] The preparation method of the Al-Mn alloy comprises the following steps:

[0029] (1) Melting: The raw material is aluminum ingots of grade AL99.70 in GB / T 1196-2008 standard, which are put into the furnace and heated to 740°C for melting;

[0030] (2) Slag removal: When the temperature is 745°C, sprinkle the slag remover evenly into the furnace and stir thoroughly for 5-10 minutes (the amount of slag remover added is 0.5kg / ton of aluminum), and use a rake to remove the slag on the surface of the aluminum liquid;

[0031] (3) Alloy: Add silicon, manganese and copper when the melt temperature is 740°C. Stir for 10-15 minutes after adding the alloy to evenly mix the components in the melt.

[0032] (4) Refining: When the melt temperature is 745°C, argon refining is adopted. High-purity argon is required, and the argon content is more than 99.7%. The refining time is 30-35 minutes. The refining agent is required to be fluorine-free and sodium-free granular refining agent, and the dosage is 1kg / ton aluminum. After refining, the scum on the liquid surface is scraped off.

[0033] (5) Standing: After refining, the melt is allowed to stand for 20 minutes;

[0034] (6) Casting: When the melt temperature is 770°C, the melt is cast into an ingot for later use;

[0035] During the casting process, Al5Ti1B aluminum titanium boron wire is added to refine the ingot grains at a rate of 75 cm / min. The ingot is degassed online on the casting launder. High-purity argon gas is introduced during degassing, and the argon content is more than 99.7%. Then, double-layer filtration (a 40ppi and a 60ppi ceramic filter plate) is used to further purify the melt. The vacuum direct cooling casting system is used for casting at a casting speed of 115±5mm / min to obtain an ingot.

[0036] (7) Homogenization: The ingot obtained above was heated to 590° C., kept at this temperature for 5 hours, and rapidly cooled to obtain a homogenized ingot;

[0037] (8) Extrusion: The short aluminum alloy round cast rod is heated and then rapidly and continuously extruded at low temperature to obtain an aluminum alloy extruded tube.

[0038] The specific implementation steps are: receive short-stock aluminum alloy round cast rods and molds → preheat the short-stock aluminum alloy round cast rods, mold barrels and molds → install extrusion molds → load short-stock aluminum alloy round cast rods → low-temperature rapid continuous extrusion → rapid cooling to obtain aluminum alloy extruded long material profiles.

[0039] Preheating conditions: Short aluminum alloy round cast bars adopt gradient preheating method, that is, the preheating temperature of the cast bars at the advanced die barrel end is high, and the preheating temperature at the backward die barrel end is low. The preheating temperature of short aluminum alloy round cast bars is 460℃ at the head, with a gradient of 3-5℃ / 100mm; the preheating temperature of the die barrel is 420-440℃, and the preheating temperature of the mold is 470℃;

[0040] Forward continuous extrusion conditions: ejector extrusion speed is 1.2-1.8 mm / s.

[0041] Example 2

[0042] An Al-Mn alloy comprises the following components by mass percentage: Si 0.48%, Fe 0.1%, Cu 0.48%, Mn 1.28%, Mg 0.02%, Zn 0.02%, Ti 0.02%, Cr 0.02%, other impurities each having a content of ≤0.05%, a total amount of impurities of ≤0.15%, and the balance being Al.

[0043] The preparation method of the Al-Mn alloy comprises the following steps:

[0044] (1) Melting: The raw material is aluminum ingots of grade AL99.70 in GB / T 1196-2008 standard, which are put into the furnace and heated to 745°C for melting;

[0045] (2) Slag removal: When the temperature is 745°C, sprinkle the slag remover evenly into the furnace and stir thoroughly for 5-10 minutes (the amount of slag remover added is 0.5kg / ton of aluminum), and use a rake to remove the slag on the surface of the aluminum liquid;

[0046] (3) Alloy: Add silicon, manganese and copper when the melt temperature is 745°C. Stir for 10-15 minutes after adding the alloy to evenly mix the components in the melt.

[0047] (4) Refining: When the melt temperature is 748°C, argon refining is adopted. High-purity argon is required, and the argon content is more than 99.7%. The refining time is 30-35 minutes. The refining agent is required to be fluorine-free and sodium-free granular refining agent, and the dosage is 1.3 kg / ton aluminum. After refining, the scum on the liquid surface is scraped off;

[0048] (5) Standing: After refining, the melt is allowed to stand for 23 minutes;

[0049] (6) Casting: When the melt temperature is 775°C, cast into ingots for later use.

[0050] During the casting process, Al5Ti1B aluminum titanium boron wire is added to refine the ingot grains at a rate of 78cm / min. Online degassing is performed on the casting launder, and high-purity argon gas is introduced during degassing, with an argon content of more than 99.7%. Then, double-layer filtration (a 40ppi and a 60ppi ceramic filter plate) is used to further purify the melt, and a vacuum direct cooling casting system is used for casting at a casting speed of 115±5mm / min to obtain an ingot.

[0051] (7) Homogenization: The ingot obtained above was heated to 595° C., kept at this temperature for 5 hours, and rapidly cooled to obtain a homogenized ingot;

[0052] (8) Extrusion: The short aluminum alloy round cast rod is heated and then rapidly and continuously extruded at low temperature to obtain an aluminum alloy extruded tube.

[0053] The specific implementation steps are: receive short-stock aluminum alloy round cast rods and molds → preheat the short-stock aluminum alloy round cast rods, mold barrels and molds → install extrusion molds → load short-stock aluminum alloy round cast rods → low-temperature rapid continuous extrusion → rapid cooling to obtain aluminum alloy extruded long material profiles.

[0054] Preheating conditions: Short-stock aluminum alloy round cast bars adopt gradient preheating method, that is, the preheating temperature of the cast bars at the advanced die barrel end is high, and the preheating temperature at the backward die barrel end is low. The preheating temperature of the short-stock aluminum alloy round cast bars is 465℃ at the head, and the cooling gradient is 3-5℃ / 100mm; the preheating temperature of the die barrel is 420-440℃, and the preheating temperature of the mold is 475℃; forward continuous extrusion conditions: the extrusion speed of the ejector rod is 1.2-1.8mm / s.

[0055] Example 3

[0056] An Al-Mn alloy comprises the following components by mass percentage: Si 0.53%, Fe 0.15%, Cu 0.5%, Mn 1.3%, Mg 0.03%, Zn 0.03%, Ti 0.02%, Cr 0.02%, other impurities each having a content of ≤0.05%, a total amount of impurities of ≤0.15%, and the balance being Al.

[0057] The preparation method of the Al-Mn alloy comprises the following steps:

[0058] (1) Melting: The raw material is aluminum ingots of grade AL99.70 in GB / T 1196-2008 standard, which are put into a furnace and heated to 750°C for melting;

[0059] (2) Slag removal: When the temperature is 745°C, sprinkle the slag remover evenly into the furnace and stir thoroughly for 5-10 minutes (the amount of slag remover added is 0.5kg / ton of aluminum), and use a rake to remove the slag on the surface of the aluminum liquid;

[0060] (3) Alloy: Add silicon, manganese and copper when the melt temperature is 750°C. After adding the alloy, stir for 10-15 minutes to evenly mix the components in the melt.

[0061] (4) Refining: When the melt temperature is 750°C, argon refining is adopted. High-purity argon is required, and the argon content is more than 99.7%. The refining time is 30-35 minutes. The refining agent is required to be fluorine-free and sodium-free granular refining agent, and the dosage is 1.3 kg / ton aluminum. After refining, the scum on the liquid surface is scraped off;

[0062] (5) Standing: After refining, the melt is allowed to stand for 25 minutes;

[0063] (6) Casting: When the melt temperature is 780°C, cast it into an ingot for later use.

[0064] During the casting process, Al5Ti1B aluminum titanium boron wire is added to refine the ingot grains at a rate of 80 cm / min. Online degassing is performed on the casting launder, and high-purity argon gas is introduced during degassing, with an argon content of more than 99.7%. Then, double-layer filtration (a 40ppi and a 60ppi ceramic filter plate) is used to further purify the melt, and a vacuum direct cooling casting system is used for casting at a casting speed of 115±5mm / min to obtain an ingot.

[0065] (7) Homogenization: The ingot obtained above was heated to 600° C., kept at this temperature for 5 hours, and rapidly cooled to obtain a homogenized ingot;

[0066] (8) Extrusion: The short aluminum alloy round cast rod is heated and then rapidly and continuously extruded at low temperature to obtain an aluminum alloy extruded tube.

[0067] The specific implementation steps are: receive short-stock aluminum alloy round cast rods and molds → preheat the short-stock aluminum alloy round cast rods, mold barrels and molds → install extrusion molds → load short-stock aluminum alloy round cast rods → low-temperature rapid continuous extrusion → rapid cooling to obtain aluminum alloy extruded long material profiles.

[0068] Preheating conditions: Short-stock aluminum alloy round cast bars adopt gradient preheating method, that is, the preheating temperature of the cast bars at the advanced die barrel end is high, and the preheating temperature at the backward die barrel end is low. The preheating temperature of the short-stock aluminum alloy round cast bars is 470℃ at the head, and the cooling gradient is 3-5℃ / 100mm; the preheating temperature of the die barrel is 420-440℃, and the preheating temperature of the mold is 480℃; forward continuous extrusion conditions: the extrusion speed of the ejector rod is 1.2-1.8mm / s.

[0069] Example 4

[0070] An Al-Mn alloy comprises the following components by mass percentage: Si 0.57%, Fe 0.25%, Cu 0.52%, Mn 1.32%, Mg 0.04%, Zn 0.02%, Ti 0.03%, Cr 0.02%, other impurities each having a content of ≤0.05%, a total amount of impurities of ≤0.15%, and the balance being Al.

[0071] The preparation method of the Al-Mn alloy comprises the following steps:

[0072] (1) Melting: The raw material is aluminum ingots of grade AL99.70 in GB / T 1196-2008 standard, which are put into the furnace and heated to 755°C for melting;

[0073] (2) Slag removal: When the temperature is 745°C, sprinkle the slag remover evenly into the furnace and stir thoroughly for 5-10 minutes (the amount of slag remover added is 0.5kg / ton of aluminum), and use a rake to remove the slag on the surface of the aluminum liquid;

[0074] (3) Alloy: Add silicon, manganese and copper when the melt temperature is 755°C. Stir for 10-15 minutes after adding the alloy to evenly mix the components in the melt.

[0075] (4) Refining: When the melt temperature is 755°C, argon refining is adopted. High-purity argon gas with an argon content of more than 99.7% is required. The refining time is 30-35 minutes. The refining agent is required to be fluorine-free and sodium-free granular refining agent with a dosage of 1.5 kg / ton aluminum. After refining, the scum on the liquid surface is scraped off;

[0076] (5) Standing: After refining, the melt is allowed to stand for 28 minutes;

[0077] (6) Casting: When the melt temperature is 785°C, cast into an ingot for later use.

[0078] During the casting process, Al5Ti1B aluminum titanium boron wire is added to refine the ingot grains at a rate of 82cm / min. Online degassing is performed on the casting launder, and high-purity argon gas is introduced during degassing, with an argon content of more than 99.7%. Then, double-layer filtration (a 40ppi and a 60ppi ceramic filter plate) is used to further purify the melt, and a vacuum direct cooling casting system is used for casting at a casting speed of 115±5mm / min to obtain an ingot.

[0079] (7) Homogenization: The ingot obtained above was heated to 605° C., kept at this temperature for 5 hours, and rapidly cooled to obtain a homogenized ingot;

[0080] (8) Extrusion: The short aluminum alloy round cast rod is heated and then rapidly and continuously extruded at low temperature to obtain an aluminum alloy extruded tube.

[0081] The specific implementation steps are: receive short-stock aluminum alloy round cast rods and molds → preheat the short-stock aluminum alloy round cast rods, mold barrels and molds → install extrusion molds → load short-stock aluminum alloy round cast rods → low-temperature rapid continuous extrusion → rapid cooling to obtain aluminum alloy extruded long material profiles.

[0082] Preheating conditions: Short-stock aluminum alloy round cast bars adopt gradient preheating method, that is, the preheating temperature of the cast bars at the advanced die barrel end is high, and the preheating temperature at the backward die barrel end is low. The preheating temperature of the short-stock aluminum alloy round cast bars is 475℃ at the head, and the cooling gradient is 3-5℃ / 100mm; the preheating temperature of the die barrel is 420-440℃, and the preheating temperature of the mold is 485℃; forward continuous extrusion conditions: the extrusion speed of the ejector rod is 1.2-1.8mm / s.

[0083] Example 5

[0084] An Al-Mn alloy comprises the following components by mass percentage: Si 0.6%, Fe 0.3%, Cu 0.55%, Mn 1.35%, Mg 0.05%, Zn 0.02%, Ti 0.02%, Cr 0.03%, other impurities each having a content of ≤0.05%, a total amount of impurities of ≤0.15%, and the balance being Al.

[0085] The preparation method of the Al-Mn alloy comprises the following steps:

[0086] (1) Melting: The raw material is aluminum ingots of grade AL99.70 in GB / T 1196-2008 standard, which are put into a furnace and heated to 760°C for melting;

[0087] (2) Slag removal: When the temperature is 745°C, sprinkle the slag remover evenly into the furnace and stir thoroughly for 5-10 minutes (the amount of slag remover added is 0.5kg / ton of aluminum), and use a rake to remove the slag on the surface of the aluminum liquid;

[0088] (3) Alloy: Add silicon, manganese and copper when the melt temperature is 760°C. After adding the alloy, stir for 10-15 minutes to evenly mix the components in the melt.

[0089] (4) Refining: When the melt temperature is 760°C, argon refining is adopted. High-purity argon gas with an argon content of more than 99.7% is required. The refining time is 30-35 minutes. The refining agent is required to be fluorine-free and sodium-free granular refining agent with a dosage of 1.5 kg / ton aluminum. After refining, the scum on the liquid surface is scraped off;

[0090] (5) Standing: After refining, the melt is allowed to stand for 30 minutes;

[0091] (6) Casting: When the melt temperature is 790°C, cast into an ingot for later use.

[0092] During the casting process, Al5Ti1B aluminum titanium boron wire is added to refine the ingot grains at a rate of 85cm / min. Online degassing is performed on the casting launder, and high-purity argon gas is introduced during degassing, with an argon content of more than 99.7%. Then, double-layer filtration (a 40ppi and a 60ppi ceramic filter plate) is used to further purify the melt, and a vacuum direct cooling casting system is used for casting at a casting speed of 115±5mm / min to obtain an ingot.

[0093] (7) Homogenization: The ingot obtained above was heated to 610° C., kept at this temperature for 5 hours, and rapidly cooled to obtain a homogenized ingot;

[0094] (8) Extrusion: The short aluminum alloy round cast rod is heated and then rapidly and continuously extruded at low temperature to obtain an aluminum alloy extruded tube.

[0095] The specific implementation steps are: receive short-stock aluminum alloy round cast rods and molds → preheat the short-stock aluminum alloy round cast rods, mold barrels and molds → install extrusion molds → load short-stock aluminum alloy round cast rods → low-temperature rapid continuous extrusion → rapid cooling to obtain aluminum alloy extruded long material profiles.

[0096] Preheating conditions: Short-stock aluminum alloy round cast bars adopt gradient preheating method, that is, the preheating temperature of the cast bars at the advanced die barrel end is high, and the preheating temperature at the backward die barrel end is low. The preheating temperature of the short-stock aluminum alloy round cast bars is 480℃ at the head, and the cooling gradient is 3-5℃ / 100mm; the preheating temperature of the die barrel is 420-440℃, and the preheating temperature of the mold is 490℃; forward continuous extrusion conditions: the extrusion speed of the ejector rod is 1.2-1.8mm / s.

[0097] Table 1 Composition of high performance Al-Mn alloys in Examples 1-3

[0098] Compare Projects Si Fe Cu Mn Mg Zn Ti Cr Al Example 1 0.45 0.05 0.45 1.25 0.01 0.01 0.01 0.01 margin Example 2 0.48 0.1 0.48 1.28 0.02 0.02 0.02 0.02 margin Example 3 0.53 0.15 0.5 1.3 0.03 0.03 0.02 0.02 margin Example 4 0.57 0.25 0.52 1.32 0.04 0.02 0.03 0.02 margin Example 5 0.6 0.3 0.55 1.35 0.05 0.02 0.02 0.03 margin

[0099] The aluminum alloy ingots of Examples 1-5 were extruded and straightened into products of the same specifications, and the thermodynamic properties were compared. The results are shown in Table 2.

[0100] Table 2 Thermodynamic properties of aluminum alloys in Examples 1-5 of the present invention

[0101] Example Tensile strength(MPa) Yield strength(MPa) Elongation(%) Example 1 168 82 27 Example 2 170 84 27 Example 3 172 86 26 Example 4 175 88 24 Example 5 178 92 24

[0102] Through the above 5 groups of embodiments, when the formula ingredients and process steps are within the protection scope of this application, the final performance of the product can meet the tensile strength ≥160MPa, yield strength ≥80MPa, and elongation ≥20%, which can meet customers' requirements for high forging performance of the product.

[0103] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. An Al-Mn alloy, characterized in that: Calculated by mass percentage, it includes the following components: Si 0.45%-0.6%, Fe≤0.3%, Cu 0.45%-0.55%, Mn 1.25%-1.35%, Mg≤0.05%, Zn≤0.1%, Ti≤0.05%, Cr≤0.05%, the individual content of other impurities ≤0.05%, the total amount of impurities ≤0.15%, and the balance is Al.

2. The method for preparing the Al-Mn alloy according to claim 1, characterized in that: The following steps are involved: (1) Melting: The raw material is aluminum ingots of grade AL99.70 in GB / T 1196-2008 standard, which are put into the furnace and heated to 730-760℃ for melting; (2) Slag removal: When the temperature is 730-760℃, sprinkle the slag remover evenly into the furnace and stir it thoroughly for 5-10 minutes. Use a rake to remove the slag on the surface of the aluminum liquid. (3) Alloy: Add silicon, manganese and copper when the melt temperature is 730-760°C. After adding the alloy, stir for 10-15 minutes to evenly mix the components in the melt. (4) Refining: When the melt temperature is 750-790°C, argon gas refining is used for 30-35 minutes. After refining, the scum on the liquid surface is removed; (5) Standing: After refining, the melt is allowed to stand for 20-30 minutes; (6) Casting: When the melt temperature is 770-790°C, it is cast into an ingot for standby use; (7) Homogenization: The ingot obtained above is heated to 600±10°C, kept at this temperature for 5-5.2 hours, and rapidly cooled to obtain a homogenized ingot; (8) Extrusion: The short aluminum alloy round cast rod is heated and then rapidly and continuously extruded at low temperature to obtain an aluminum alloy extruded tube billet.

3. The method for preparing the Al-Mn alloy according to claim 2, characterized in that: The amount of slag remover added in step (2) is 0.5 kg / ton of aluminum.

4. The method for preparing the Al-Mn alloy according to claim 2, characterized in that: During the refining in step (4), argon gas with a purity of more than 99.7% is introduced; the refining agent used during the refining is a fluorine-free and sodium-free granular refining agent, and the amount used is 1-1.5 kg / ton of aluminum.

5. The method for preparing the Al-Mn alloy according to claim 2, characterized in that: In step (5), during the casting process, Al5Ti1B aluminum titanium boron wire is added to refine the ingot grains, and the addition rate is 75-85 cm / min. Online degassing is performed on the casting launder. High-purity argon gas is introduced during degassing, and the argon content is more than 99.7%. Then, double-layer filtration is used to further purify the melt. The casting is performed using a vacuum direct cooling casting system, and the casting rate is 115±5 mm / min. Finally, an ingot is obtained.

6. The method for preparing the Al-Mn alloy according to claim 2, characterized in that: The specific steps of extrusion in step (7) are as follows: obtaining short-stock aluminum alloy round cast rods and molds → preheating the short-stock aluminum alloy round cast rods, mold barrels and molds → installing extrusion molds → loading short-stock aluminum alloy round cast rods → low-temperature rapid continuous extrusion → water cooling to obtain aluminum alloy extruded long material profiles.

7. The method for preparing the Al-Mn alloy according to claim 6, characterized in that: The short-stock aluminum alloy round cast rod adopts a gradient preheating method: the preheating temperature of the cast rod at the advanced die barrel end is high, and the preheating temperature at the backward die barrel end is low. The preheating temperature of the head of the short-stock aluminum alloy round cast rod is 460-480°C, and the decreasing gradient is 3-5°C / 100 mm; The preheating temperature of the mold barrel is 420-440°C; The preheating temperature of the mold is 470-490°C.

8. The method for preparing the Al-Mn alloy according to claim 6, characterized in that: Continuous extrusion conditions: ejector extrusion speed is 1.2-1.8 mm / s, extrusion temperature is 420-440°C.