Aluminum alloy powder for additive manufacturing, additive manufacturing method and heat dissipation component
By adding elements such as Ni, Fe, Zr, Sc to the aluminum alloy powder, combined with additive manufacturing forming and heat treatment technology, the problems of low thermal conductivity and cracks in aluminum alloy materials in additive manufacturing are solved, and high thermal conductivity and good thermal conductivity are achieved Aluminum alloy material with mechanical properties is suitable for the preparation of heat dissipation components in complex shapes.
Patent Information
- Application Number
- CN202411034058.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
AI Technical Summary
The existing aluminum alloy materials for additive manufacturing have low thermal conductivity, and there are cracks that are difficult to eliminate after forming through additive manufacturing, resulting in low mechanical properties and thermal conductivity, making it difficult to meet the requirements of heat dissipation parts in the aerospace field.
By adding Ni, Fe, Zr, Sc and other elements to aluminum alloy powder, combined with additive manufacturing forming and heat treatment technology, the degree of alloying is reduced, lattice distortion and tissue defects are reduced, and the stable dispersion phase is formed, and the mechanical strength of the material is improved. and thermal conductivity.
It achieves high thermal conductivity and good mechanical properties, provides high thermal conductivity aluminum alloy materials suitable for additive manufacturing, suitable for the preparation of heat dissipation components in complex shapes, and meets the thermal management needs of the aerospace field.
Smart Images

Figure CN118932222A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal additive manufacturing, and in particular to an aluminum alloy powder for additive manufacturing, an additive manufacturing method and a heat dissipation component. Background Art
[0002] Additive manufacturing technology is a new type of digital processing technology that uses high-energy heat sources to melt powder or wire, and then prints layer by layer according to the three-dimensional discrete data of the parts to finally obtain the parts. It has the advantages of design freedom, integration, lightweight, complex structure, short development cycle and low cost. It is widely used in the preparation of complex, lightweight and functional components in the fields of aerospace, rail transportation, automobiles and ships. It is also increasingly used in the field of thermal management, such as producing lighter and smaller heat exchangers with complex geometric shapes and large surface areas, producing heat pipes with complex internal cooling channels, and topologically optimized radiators with high heat dissipation efficiency.
[0003] At present, the commonly used heat dissipation materials are mainly copper alloys and aluminum alloys. For the aerospace field, aluminum alloy is the preferred material for heat dissipation components, taking into account the characteristics of lightweight and high thermal conductivity. The aluminum alloy materials used for additive manufacturing are mainly AlSi 10 Mg, AlSi7Mg, AlSi 12 , high-strength AlSc alloy powder, etc., but the thermal conductivity of the above-mentioned aluminum alloy materials is poor, and their thermal conductivity is difficult to stably reach above 150W / (m·K). Existing mature aluminum alloy materials, such as 6061, 6063, etc., although the thermal conductivity after forming by traditional processes is in the range of 180~200W / (m·K), but these materials have cracks that are difficult to eliminate after forming by additive manufacturing, resulting in the mechanical properties and thermal conductivity of the formed parts being lower than those prepared by traditional processes, and it is difficult to meet the requirements of heat dissipation parts. In summary, the lack of high thermal conductivity aluminum alloy powder materials suitable for additive manufacturing has limited the application of additive manufacturing technology in the field of thermal management, so it is urgent to develop a new high thermal conductivity aluminum alloy material and preparation process to solve this problem. Summary of the invention
[0004] In view of the problem that there are few types of aluminum alloy materials for additive manufacturing and their low thermal conductivity, the present invention provides an aluminum alloy powder for additive manufacturing, an additive manufacturing method and a heat dissipation component. Through technical means such as material composition design, additive manufacturing forming process and heat treatment, the degree of alloying, lattice distortion and structural defects are reduced as much as possible to achieve a comprehensive improvement in the strength and thermal conductivity of the material.
[0005] The present invention includes an aluminum alloy powder for additive manufacturing, which contains the following components in mass percentage: Al≥93.5wt.%, Ni: 0.01-2wt.%, Fe: 0-1wt.%, Zr: 0.1-2wt.%, Sc: 0-1wt.%, and inevitable impurities.
[0006] Furthermore, the particle size distribution range of the aluminum alloy powder is D10 ≥ 10 μm, D90: ≤ 75 μm.
[0007] Furthermore, the bulk density of the aluminum alloy powder is ≥1.2g / cm 3 , powder tap density ≥1.5g / cm 3 .
[0008] As a general inventive concept, it also includes an additive manufacturing method, comprising the following steps:
[0009] S1. Blending elements according to the designed composition to prepare an aluminum alloy powder for additive manufacturing as described above;
[0010] S2, construct a three-dimensional model of the target component, import the support of the three-dimensional model, and input it into the laser selective melting forming equipment after two-dimensional slicing;
[0011] S3, setting the processing parameters of laser selective melting, including laser power, powder layer thickness, scanning rate and scanning spacing, and performing laser selective melting processing;
[0012] S4. The formed part obtained in S3 is subjected to heat treatment, wire cutting and surface treatment.
[0013] Furthermore, in S1, the preparation process of the aluminum alloy powder specifically includes at least one of gas atomization, rotating electrode atomization, plasma atomization, ultrasonic atomization and rotating disk atomization;
[0014] In S1, the prepared aluminum alloy powder is further dried at a temperature of 600 to 100° C. for a drying time of 4 to 12 hours.
[0015] Furthermore, in S2, the thickness of the two-dimensional slice is 0.03-0.06 mm.
[0016] Furthermore, in S3, the laser power is 250-500 W, the powder layer thickness is 30-60 μm, the scanning rate is 800-1400 mm / s, and the scanning interval is 90-130 μm.
[0017] Furthermore, in S4, the heat treatment includes:
[0018] Stress relief annealing, temperature is 150-250℃, holding time is 2-4h, heating rate is 5-10℃ / min;
[0019] The second stage annealing, the temperature is 300 ~ 500 ℃, the holding time is 4 ~ 24h, the heating rate is 5 ~ 10 ℃ / min;
[0020] Then cool in the furnace.
[0021] Furthermore, in S4, the surface treatment includes surface cleaning, surface grinding and polishing, and surface sandblasting;
[0022] The surface cleaning is ultrasonic cleaning, using anhydrous ethanol as the cleaning medium, and the cleaning time is 10 to 60 minutes;
[0023] The surface sandblasting uses corundum sand as the medium, and the particle size of corundum sand is 0.5-1mm;
[0024] Surface grinding and polishing: Grind on #600, #1000, #2000, and #3000 sandpaper in sequence until the surface is flat and smooth.
[0025] As a general inventive concept, it also includes a heat dissipation component, which is prepared using any of the aluminum alloy powders for additive manufacturing as described above, or prepared by any of the additive manufacturing methods as described above.
[0026] Beneficial effects of the present invention:
[0027] The aluminum alloy powder formula for additive manufacturing and the additive manufacturing method provided by the present invention can avoid the increase in thermal resistance of the aluminum alloy structure caused by element solid solution and second phase precipitation, and to a certain extent, reduce internal defects such as cracks, looseness, shrinkage holes, etc. through forming, thereby improving the overall comprehensive performance of the material.
[0028] The present invention provides an aluminum alloy powder for additive manufacturing, wherein Fe, Ni, Zr, Sc and the like are selected as main strengthening elements, and the diffusion coefficient of the elements in the aluminum alloy matrix is low, and a stable dispersed phase can be formed to refine the grains, thereby enhancing the mechanical strength of the material. Meanwhile, the low addition of elements can avoid a significant reduction in the thermal conductivity of the material. Through the additive manufacturing forming and heat treatment process of the present invention, a high thermal conductivity aluminum alloy part with relatively dense structure, few defects and good comprehensive performance is finally obtained.
[0029] The present invention mainly reduces the degree of alloying, lattice distortion, and structural defects as much as possible through technical means such as material composition design, additive manufacturing forming process, and heat treatment, so as to achieve a comprehensive improvement in the strength and thermal conductivity of the material.
[0030] The aluminum alloy powder for additive manufacturing and the additive manufacturing method provided by the present invention are suitable for preparing aluminum alloy heat dissipation components. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Attached Figure 1 This is a 500x SEM image of the aluminum alloy powder in Example 1 of the present invention;
[0032] Attached Figure 2 This is a 10000x SEM image of the aluminum alloy powder in Example 1 of the present invention;
[0033] Attached Figure 3 This is a micrograph of the structure of the aluminum alloy of the additively manufactured product in Example 1 of the present invention;
[0034] Attached Figure 4 This is a micrograph of the structure of the aluminum alloy of the additively manufactured product in Example 2 of the present invention;
[0035] Attached Figure 5 This is a micrograph of the structure of the aluminum alloy product manufactured by additive manufacturing in Example 3 of the present invention. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific implementation methods. It should be understood that the specific implementation methods described herein are only used to explain the present invention and are not intended to limit the present invention.
[0037] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items. In addition, the technical solutions between the various embodiments of the present invention can be combined with each other, but it must be based on the ability of ordinary technicians in the field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0038] The embodiment of the present invention provides an aluminum alloy powder for additive manufacturing, wherein the aluminum alloy powder contains the following components in mass percentage: Al ≥ 93.5wt.%, Ni: 0.01-2wt.%, Fe: 0-1wt.%, Zr: 0.1-2wt.%, Sc: 0-1wt.%, and unavoidable impurities; a single type of impurity element in the impurities is ≤ 0.1wt.%, and the total amount of impurity elements is ≤ 0.2wt.%. In addition, other strengthening alloy elements other than Fe, Ni, Zr, and Sc, such as Mn, Si, Ti or other rare earth elements, etc., may be added to the aluminum alloy powder for additive manufacturing, but these strengthening alloy elements are not elements that are intentionally added and designed to be proportioned in the technical solution of the present invention, and can be avoided or removed in the process of preparing the alloy, and it is necessary to ensure that the single type of metal elements of other strengthening metal elements is ≤ 0.1wt.%, and the total content does not exceed 0.3wt.%.
[0039] At present, the aluminum alloys suitable for additive manufacturing are mainly AlSi 10 Mg, AlSi7Mg, AlSi 12 , high-strength AlSc alloy powder, etc., but their thermal conductivity is relatively low. In order to improve the performance of aluminum alloys for additive manufacturing, it is generally strengthened by introducing elements such as Ti, Sc, Ni, Cu and the second phase into the aluminum alloy matrix. However, the present invention has found that since the alloy elements will form a solid solution or produce a precipitation phase while improving the strength and weldability, the solid solution will cause the lattice distortion phase of the aluminum matrix and introduce a new interface, and the precipitation phase will aggravate the scattering of heat in the process of lattice vibration conduction, thereby hindering the thermal conductivity of the overall material. The aluminum alloy materials reported by the invention all show lower thermal conductivity than before the strengthening treatment; the aluminum alloy powder formula for additive manufacturing and the additive manufacturing method provided by the present invention can avoid the increase of the thermal resistance of the aluminum alloy structure caused by the solid solution of elements and the precipitation of the second phase, and to a certain extent, reduce the internal cracks, looseness, shrinkage holes and other defects through forming, thereby improving the overall comprehensive performance of the material;
[0040] The aluminum alloy powder for additive manufacturing provided in an embodiment of the present invention selects Fe, Ni, Zr, Sc, etc. as main strengthening elements. The diffusion coefficient of these elements in the aluminum alloy matrix is low, and a stable dispersed phase can be formed to refine the grains and enhance the mechanical strength of the material. At the same time, the low element addition can avoid a significant reduction in the thermal conductivity of the material. The Ni content in the present invention is in the range of 0.01-2wt.%, and the Fe content is in the range of 0-1wt.%. The addition of Ni and Fe can effectively improve the tensile strength, yield strength and high-temperature stability of the aluminum alloy material, and ensure the thermal conductivity of the material at room temperature and high temperature. However, when the Ni and Fe content is too high, more brittle second phases will be precipitated during the heat treatment process, affecting the elongation and thermal conductivity of the material. Therefore, a certain amount of Ni and Fe elements are selected to ensure the comprehensive performance of the material; and Zr and Sc are strengthening additive elements that can effectively improve the mechanical properties of the aluminum alloy. Within a certain content range, the mechanical properties of the material as a whole can be improved, while the thermal conductivity is less reduced; according to the material ratio design in the present invention, combined with the additive manufacturing forming and heat treatment process, a high thermal conductivity aluminum alloy part with relatively dense structure, few defects and good comprehensive performance is finally obtained.
[0041] In a preferred embodiment, the selected aluminum alloy powder is subjected to mechanical ultrasonic vibration screening, the mesh size of the screen is 200-300 mesh, the powder is dispersed, and the aluminum alloy powder particle size distribution range is D10 ≥ 10 μm, D90: ≤ 75 μm. In this particle size distribution range, the aluminum alloy powder has a higher forming density, fewer defects, and more stable mechanical properties and thermal conductivity of the formed part. In the particle size range outside the scope of the embodiment of the present invention, the powder has a higher impurity content, more forming defects, and poor forming quality, making it difficult to ensure the performance stability of the product.
[0042] In a preferred embodiment, the bulk density of the aluminum alloy powder is ≥1.2 g / cm 3 , powder tap density ≥1.5g / cm 3 , ensuring the fluidity of the powder to be suitable for additive manufacturing forming process.
[0043] The embodiment of the present invention further provides an additive manufacturing method, comprising the following steps:
[0044] S1. balancing the elements according to the designed composition to prepare the aluminum alloy powder for additive manufacturing as described above;
[0045] S2. Use 3D modeling software to build a 3D model of the target component, import the 3D model into supports, slice it in 2D, and then input it into the laser selective melting forming equipment;
[0046] S3, setting processing parameters of the laser selective melting process, including laser power, powder layer thickness, scanning rate and scanning spacing, and performing laser selective melting to obtain a formed part;
[0047] S4, subjecting the formed part obtained in S3 to heat treatment, wire cutting and surface treatment to obtain a finished product of the target component.
[0048] In a preferred embodiment, in S1, the preparation process of the aluminum alloy powder specifically includes at least one of gas atomization, rotating electrode atomization, plasma atomization, ultrasonic atomization and rotating disk atomization to obtain a high thermal conductivity aluminum alloy powder raw material with uniform composition, low impurity content and good fluidity.
[0049] In S1, the prepared aluminum alloy powder is also dried to remove the moisture adsorbed in the powder to ensure the quality stability of the aluminum alloy powder during the additive manufacturing process; specifically, vacuum drying is performed in a drying oven with a vacuum degree of 10 -1 Pa or less, to ensure the oxidation reaction on the surface of the aluminum alloy powder during the drying process and reduce the increase in oxygen content, the drying temperature is 60-100°C, and the drying time is 4-12h. Higher temperature and longer drying time will cause the aluminum alloy powder to react, introduce impurities, and increase production costs. The processing method of the present invention can completely dry the aluminum alloy powder and remove residual moisture in the clean powder to ensure the printing quality.
[0050] In a preferred embodiment, in S2, specifically, the required model is constructed using 3D software and saved in STL format, and the constructed model is further supported and sliced in two dimensions by additive manufacturing processing software; the thickness of the two-dimensional slice is 0.03-0.06 mm. Within this thickness range, the material forming efficiency and performance can be comprehensively considered; among which, a lower forming thickness can improve the accuracy of the material, but it will reduce the forming efficiency of the material, and a higher forming thickness, although it can improve the forming efficiency, due to the limitations of laser power and forming technology, the forming accuracy of the material is poor, and it is difficult to meet the general material internal and external quality requirements.
[0051] In a preferred embodiment, in the forming process parameters of S3, the laser power is 250-500W, the powder layer thickness is 30-60μm, the scanning rate is 800-1400mm / s, and the scanning spacing is 90-130μm; the performance of the formed parts obtained in the above preparation process is relatively stable, and in the rapid laser melting and condensation process, it can avoid stress defects caused by volume shrinkage, reduce cracks and gaps, and prevent serious specimen fracture cracks.
[0052] In a preferred embodiment, in S3, the hot aluminum alloy powder laser selective melting forming process is always in an argon protection state, and the oxygen content in the forming chamber does not exceed 0.1%, ensuring that during the forming process, the increase in impurity oxygen content is reduced and the safety of production and manufacturing is improved.
[0053] In a preferred embodiment, in S3, the substrate used in laser selective melting is a 2 / 6 series aluminum alloy plate, and the preset temperature is 60-100°C; the substrate material and preset temperature selected in the embodiment of the present invention can be more completely melted with the thermal conductive aluminum alloy powder in the early stage of the forming process, thereby avoiding warping or fracture of the material due to defects and stress in subsequent aluminum alloy forming.
[0054] In a preferred embodiment, in S4, the specific process of heat treatment is: stress relief annealing, the temperature is 150-250°C, the holding time is 2-4h, and the heating rate is 5-10°C / min; the second stage annealing, the temperature is 300-500°C, the holding time is 4-24h, and the heating rate is 5-10°C / min; then cooled with the furnace; the purpose of heat treatment in the embodiment of the present invention is to improve the comprehensive performance of the material; stress relief annealing can eliminate the large stress formed by the rapid condensation of metal in the additive manufacturing process of aluminum alloy materials, thereby improving the elongation of the material; the second stage annealing can improve the aluminum alloy structure, disperse and precipitate AlNi, AlFe, AlZr, AlSc phases, and strengthen the material performance; the heat treatment temperature range in the embodiment of the present invention can effectively precipitate the strengthening elements dissolved in the aluminum alloy, disperse them at the grain boundaries, play a strengthening role, and ensure the mechanical properties and thermal conductivity of the material.
[0055] In a preferred embodiment, in S4, the surface treatment includes surface cleaning, surface grinding and polishing, and surface sandblasting; wherein, the surface cleaning is ultrasonic cleaning, using anhydrous ethanol as the cleaning medium, and the cleaning time is 10 to 60 minutes; the surface sandblasting uses corundum sand as the medium, and the corundum sand has a particle size of 0.5 to 1 mm; the surface grinding and polishing is performed on #600, #1000, #2000, and #3000 sandpaper in sequence until the surface is flat and smooth.
[0056] In a preferred embodiment, in S4, the wire cutting is specifically a repeated wire electric spark wire cutting machine tool, which is performed at a speed lower than 10 mm / s to avoid warping and deformation of the additively manufactured part.
[0057] The embodiment of the present invention further provides a heat dissipation component, which is prepared by using the aluminum alloy powder for additive manufacturing as described above, or by using the additive manufacturing method as described above. The aluminum alloy component prepared by the embodiment of the present invention has high strength and good thermal conductivity.
[0058] Example 1
[0059] This embodiment provides an additive manufacturing method, comprising the following steps:
[0060] S1. A high thermal conductivity aluminum alloy powder is prepared by gas atomization as a raw material for additive manufacturing. The main components of the powder are Ni: 0.3wt%, Zr: 0.5wt%, Fe: 0.2wt%, O≤0.15wt%, other elements≤0.1wt%, Al: ≥98.7%; the powder particle size distribution is D10: 22μm, D50: 35μm, D90: 62μm, and the powder bulk density is 1.32g / cm 3 , the powder tap density is 1.53g / cm 3 , suitable for additive manufacturing forming process;
[0061] S2. Use SolidWorks / UG 3D modeling software to build the required target structure part model, import the model for support, slice it in two dimensions (0.03mm), and then input it into the laser selective melting molding equipment;
[0062] S3. Use additive manufacturing forming equipment for forming processing. Before starting, ensure that the raw material powder in the powder chamber is sufficient, the substrate preheating temperature is 80°C, and argon is introduced into the forming chamber as a protective gas to ensure that the oxygen content is less than 0.1%; set the relevant printing parameters, the laser power is 460W, the powder layer thickness is 30μm, the scanning rate is 900mm / s, and the scanning interval is 120μm;
[0063] S4. Take out the printed aluminum alloy parts and perform heat treatment with the substrate. The stress relief annealing temperature is 240℃, the holding time is 2h, the heating rate is 10℃ / min, the second annealing temperature range is 420℃, the holding time is 4h, the heating rate is 10℃ / min, and then cool with the furnace; after cooling to room temperature, use the electric spark wire cutting machine to perform wire cutting; then use anhydrous ethanol to clean the formed parts and sandblast the surface, and use #600, #1000, #2000, and #3000 sandpaper to polish them in turn until the surface is flat and smooth, and test its performance by machine-added tensile parts;
[0064] In this embodiment, the room temperature tensile strength of the laser selective melting formed part reaches 310MPa, the elongation reaches 8%, and the thermal conductivity reaches 198W / (m·K). Figure 1 and attached Figure 2 As shown in the attached figure, the high thermal conductivity aluminum alloy powder of the present invention has high sphericity and good fluidity, and the powder particle size is basically in the range of 15 to 70 μm; Figure 3 As shown, the high thermal conductivity aluminum alloy powder has fewer structural defects and higher density after forming.
[0065] Example 2
[0066] This embodiment provides an additive manufacturing method, comprising the following steps:
[0067] S1. Select high thermal conductivity aluminum alloy powder as the raw material for additive manufacturing. The main components of the powder are Ni: 0.5wt%, Zr: 0.7wt%, O≤0.15wt%, other elements ≤0.1wt%, Al: ≥98.5%; the powder particle size distribution is D10: 23μm, D50: 36μm, D90: 64μm, and the powder bulk density is 1.34g / cm 3 , the powder tap density is 1.57g / cm 3 , suitable for additive manufacturing forming process;
[0068] S2. Use SolidWorks / UG 3D modeling software to build the required target structure part model, import the model for support, slice it in two dimensions (0.03mm), and then input it into the laser selective melting molding equipment;
[0069] S3. Use additive manufacturing forming equipment for forming processing. Before starting, ensure that the raw material powder in the powder chamber is sufficient, the substrate preheating temperature is 80°C, and argon is introduced into the forming chamber as a protective gas to ensure that the oxygen content is less than 0.1%; set the relevant printing parameters, the laser power is 480W, the powder layer thickness is 30μm, the scanning rate is 1000mm / s, and the scanning interval is 110μm;
[0070] S4. Take out the printed aluminum alloy parts and perform heat treatment with the substrate. The stress relief annealing temperature is 240℃, the holding time is 2h, the heating rate is 10℃ / min, the second annealing temperature range is 420℃, the holding time is 12h, the heating rate is 10℃ / min, and then cool with the furnace; after cooling to room temperature, use the electric spark wire cutting machine to perform wire cutting; then use anhydrous ethanol to clean the formed parts and sandblast the surface, and use #600, #1000, #2000, and #3000 sandpaper to polish them in turn until the surface is flat and smooth, and test the performance of the machined tensile parts;
[0071] In this embodiment, the room temperature tensile strength of the laser selective melting formed part reaches 308MPa, the elongation reaches 10%, and the thermal conductivity reaches 212W / (m·K). Figure 4 As shown, the high thermal conductivity aluminum alloy powder has fewer structural defects and higher density after forming.
[0072] Example 3
[0073] This embodiment provides an additive manufacturing method, comprising the following steps:
[0074] S1. Select high thermal conductivity aluminum alloy powder as the raw material for additive manufacturing. The main components of the powder are Ni: 1.0wt%, Zr: 1.0wt%, Sc: 0.1wt%, O≤0.15wt%, other elements≤0.1wt%, Al: ≥97.7%; the powder particle size distribution is D10: 22μm, D50: 35μm, D90: 61μm, and the powder bulk density is 1.31g / cm 3 , the powder tap density is 1.54g / cm 3 , suitable for additive manufacturing forming process;
[0075] S2. Use SolidWorks / UG 3D modeling software to build the required target structure part model, import the model for support, slice it in two dimensions (0.03mm), and then input it into the laser selective melting molding equipment;
[0076] S3. Use additive manufacturing forming equipment for forming processing. Before starting, ensure that the raw material powder in the powder chamber is sufficient, the substrate preheating temperature is 80°C, and argon is introduced into the forming chamber as a protective gas to ensure that the oxygen content is less than 0.1%; set the relevant printing parameters, the laser power is 460W, the powder layer thickness is 30μm, the scanning rate is 900mm / s, and the scanning interval is 120μm;
[0077] S4. Take out the printed aluminum alloy parts and perform heat treatment with the substrate. The stress relief annealing temperature is 240℃, the holding time is 2h, the heating rate is 10℃ / min, the second annealing temperature range is 420℃, the holding time is 4h, the heating rate is 10℃ / min, and then cool with the furnace; after cooling to room temperature, use electric spark wire cutting machine to cut the wire; then use anhydrous ethanol to clean the formed parts and sandblast the surface, and use #600, #1000, #2000, and #3000 sandpaper to polish them in turn until the surface is flat and smooth, and test its performance by machined tensile parts.
[0078] In this embodiment, the room temperature tensile strength of the laser selective melting formed part reaches 350MPa, the elongation reaches 8%, and the thermal conductivity reaches 191W / (m·K). Figure 5 As shown, the high thermal conductivity aluminum alloy powder has fewer structural defects after forming, compared with more structural defects in Examples 1 and 2.
[0079] Comparative Example 1
[0080] This comparative example provides an AlSi series aluminum alloy additive manufacturing method, comprising the following steps:
[0081] S1. AlSi aluminum alloy powder is selected as the raw material for additive manufacturing. The main components of the powder are Si: 10wt%, Mg: 0.3wt%, O≤0.15wt%, other elements≤0.1wt%, Al: ≥89.4%; the powder particle size distribution is D10: 20μm, D50: 34μm, D90: 58μm, and the powder bulk density is 1.3g / cm 3 , the powder tap density is 1.5g / cm 3 , suitable for additive manufacturing forming process;
[0082] S2. Use SolidWorks / UG 3D modeling software to build the required target structure part model, import the model for support, slice it in two dimensions (0.03mm), and then input it into the laser selective melting molding equipment;
[0083] S3. Use additive manufacturing forming equipment for forming processing. Before starting, ensure that the raw material powder in the powder chamber is sufficient, the substrate preheating temperature is 80°C, and argon is introduced into the forming chamber as a protective gas to ensure that the oxygen content is less than 0.1%; set the relevant printing parameters, the laser power is 400W, the powder layer thickness is 30μm, the scanning rate is 1000mm / s, and the scanning interval is 120μm;
[0084] S4. Take out the printed aluminum alloy parts and perform heat treatment with the substrate. The stress relief annealing temperature is 300℃, the holding time is 2h, the heating rate is 10℃ / min, and then it is cooled with the furnace; after it cools to room temperature, it is cut by an electric spark wire cutting machine; then, anhydrous ethanol is used to clean and sandblast the formed parts, and #600, #1000, #2000, and #3000 sandpaper are used to polish them in turn until the surface is flat and smooth, and the performance of the machined tensile parts is tested.
[0085] The room temperature tensile strength of the laser selective melting formed part in this comparative example reaches 300 MPa, the elongation reaches 8%, and the thermal conductivity reaches 140 W / (m·K). Compared with the high thermal conductivity aluminum alloy in the embodiment of the present invention, its mechanical properties are similar, but its thermal conductivity is poor.
[0086] Comparative Example 2
[0087] This comparative example provides an additive manufacturing method, comprising the following steps:
[0088] S1. Select high thermal conductivity aluminum alloy powder as the raw material for additive manufacturing. The main components of the powder are Ni: 3wt%, Zr: 3wt%, O≤0.15wt%, other elements≤0.1wt%, Al: ≥93.7%; the powder particle size distribution is D10: 23μm, D50: 36μm, D90: 64μm, and the powder bulk density is 1.34g / cm 3, the powder tap density is 1.57g / cm 3 , suitable for additive manufacturing forming process;
[0089] S2. Use SolidWorks / UG 3D modeling software to build the required target structure part model, import the model for support, slice it in two dimensions (0.03mm), and then input it into the laser selective melting molding equipment;
[0090] S3. Use additive manufacturing forming equipment for forming processing. Before starting, ensure that the raw material powder in the powder chamber is sufficient, the substrate preheating temperature is 80°C, and argon is introduced into the forming chamber as a protective gas to ensure that the oxygen content is less than 0.1%; set the relevant printing parameters, the laser power is 480W, the powder layer thickness is 30μm, the scanning rate is 1000mm / s, and the scanning interval is 110μm;
[0091] S4. Take out the printed aluminum alloy parts and perform heat treatment with the substrate. The stress relief annealing temperature is 240℃, the holding time is 2h, the heating rate is 10℃ / min, the second annealing temperature range is 420℃, the holding time is 12h, the heating rate is 10℃ / min, and then cool with the furnace; after cooling to room temperature, use the electric spark wire cutting machine to perform wire cutting; then use anhydrous ethanol to clean the formed parts and sandblast the surface, and use #600, #1000, #2000, and #3000 sandpaper to polish them in turn until the surface is flat and smooth, and test the performance of the machined tensile parts;
[0092] In this comparative example, the room temperature tensile strength of the laser selective melting formed part reaches 280MPa, the elongation reaches 4%, and the thermal conductivity reaches 185W / (m·K). Compared with the embodiment of the present invention, the excessive addition of Ni and Zr leads to element segregation, precipitation of harmful second phase, and reduction of mechanical properties and thermal conductivity of the material.
[0093] Comparative Example 3
[0094] This comparative example provides an additive manufacturing method, comprising the following steps:
[0095] S1. Select high thermal conductivity aluminum alloy powder as the raw material for additive manufacturing. The main components of the powder are Fe: 0.5wt%, Zr: 0.7wt%, O≤0.15wt%, other elements ≤0.1wt%, Al: ≥98.5%; the powder particle size distribution is D10: 23μm, D50: 36μm, D90: 64μm, and the powder bulk density is 1.34g / cm 3 , the powder tap density is 1.57g / cm 3 , suitable for additive manufacturing forming process;
[0096] S2. Use SolidWorks / UG 3D modeling software to build the required target structure part model, import the model for support, slice it in two dimensions (0.03mm), and then input it into the laser selective melting molding equipment;
[0097] S3. Use additive manufacturing forming equipment for forming processing. Before starting, ensure that the raw material powder in the powder chamber is sufficient, the substrate preheating temperature is 80°C, and argon is introduced into the forming chamber as a protective gas to ensure that the oxygen content is less than 0.1%; set the relevant printing parameters, the laser power is 240W, the powder layer thickness is 80μm, the scanning rate is 1600mm / s, and the scanning interval is 110μm;
[0098] S4. Take out the printed aluminum alloy parts and perform heat treatment with the substrate. The stress relief annealing temperature is 240℃, the holding time is 2h, the heating rate is 10℃ / min, the second annealing temperature range is 420℃, the holding time is 12h, the heating rate is 10℃ / min, and then cool with the furnace; after cooling to room temperature, use the electric spark wire cutting machine to perform wire cutting; then use anhydrous ethanol to clean the formed parts and sandblast the surface, and use #600, #1000, #2000, and #3000 sandpaper to polish them in turn until the surface is flat and smooth, and test the performance of the machined tensile parts;
[0099] The room temperature tensile strength of the laser selective melting formed part in this comparative example reaches 150MPa, the elongation reaches 5%, and the thermal conductivity reaches 140W / (m·K). This comparative example adopts parameters outside the forming process range of the present invention, resulting in increased material defects and reduced mechanical properties and thermal conductivity of the material.
[0100] Comparative Example 4
[0101] This comparative example provides an additive manufacturing method, comprising the following steps:
[0102] S1. Select high thermal conductivity aluminum alloy powder as the raw material for additive manufacturing. The main components of the powder are Ni: 0.5wt%, Zr: 0.7wt%, O≤0.15wt%, other elements ≤0.1wt%, Al: ≥98.5%; the powder particle size distribution is D10: 23μm, D50: 36μm, D90: 64μm, and the powder bulk density is 1.34g / cm 3 , the powder tap density is 1.57g / cm 3 , suitable for additive manufacturing forming process;
[0103] S2. Use SolidWorks / UG 3D modeling software to build the required target structure part model, import the model for support, slice it in two dimensions (0.03mm), and then input it into the laser selective melting molding equipment;
[0104] S3. Use additive manufacturing forming equipment for forming processing. Before starting, ensure that the raw material powder in the powder chamber is sufficient, the substrate preheating temperature is 80°C, and argon is introduced into the forming chamber as a protective gas to ensure that the oxygen content is less than 0.1%; set the relevant printing parameters, the laser power is 480W, the powder layer thickness is 30μm, the scanning rate is 1000mm / s, and the scanning interval is 110μm;
[0105] S4. Take out the printed aluminum alloy parts and perform heat treatment with the substrate. The stress relief annealing temperature is 240℃, the holding time is 2h, the heating rate is 10℃ / min, and then it is cooled with the furnace; after it is cooled to room temperature, it is cut by an electric spark wire cutting machine; then anhydrous ethanol is used to clean the formed parts and the surface is sandblasted, and #600, #1000, #2000, and #3000 sandpaper are used to polish it in turn until the surface is flat and smooth, and the performance of the machined tensile parts is tested;
[0106] The room temperature tensile strength of the laser selective melting formed part in this comparative example reaches 360MPa, the elongation reaches 8%, and the thermal conductivity reaches 150W / (m·K). Compared with the high thermal conductivity aluminum alloy in Example 2 of the present invention, the present comparative example has incomplete precipitation of the dispersed phase in the internal structure of the material due to the different heat treatment method. Although the mechanical properties are improved due to the internal stress or oversolid solution strengthening effect, the thermal conductivity of the material is greatly reduced.
[0107] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0108] The above-mentioned embodiments only express several implementation modes of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention. It should be pointed out that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the attached claims.
[0109] The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.
Claims
1. An aluminum alloy powder for additive manufacturing, It is characterized in that The aluminum alloy powder contains the following components in percentage by mass: Al≥93.5wt.% Ni: 0.01~2wt.% Fe: 0~1wt.% Zr: 0.1~2wt.% Sc: 0~1wt.% and inevitable impurities.
2. The aluminum alloy powder for additive manufacturing according to claim 1, It is characterized in that The particle size distribution range of the aluminum alloy powder is D10≥10μm, D90:≤75μm.
3. The aluminum alloy powder for additive manufacturing according to claim 1, It is characterized in that The bulk density of the aluminum alloy powder is ≥1.2 g / cm 3 , powder tap density ≥1.5g / cm 3 .
4. An additive manufacturing method, It is characterized in that The following steps are involved: S1. Mixing elements according to the designed composition to prepare the aluminum alloy powder for additive manufacturing as claimed in any one of claims 1 to 3; S2, constructing a three-dimensional model of the target component, and importing the three-dimensional model for support, slicing it in two dimensions, and then inputting it into a laser selective melting forming device; S3, setting the processing parameters of laser selective melting, including laser power, powder layer thickness, scanning rate and scanning spacing, and performing laser selective melting processing; S4, subjecting the formed part obtained in S3 to heat treatment, wire cutting and surface treatment.
5. The additive manufacturing method according to claim 4, It is characterized in that In S1, the preparation process of the aluminum alloy powder specifically includes at least one of gas atomization, rotating electrode atomization, plasma atomization, ultrasonic atomization and rotating disk atomization.
6. The additive manufacturing method according to claim 4, It is characterized in that In S2, the thickness of the two-dimensional slice is 0.03-0.06 mm.
7. The additive manufacturing method according to claim 4, It is characterized in that In S3, the laser power is 250-500 W, the powder layer thickness is 30-60 μm, the scanning rate is 800-1400 mm / s, and the scanning interval is 90-130 μm.
8. The additive manufacturing method according to claim 4, It is characterized in that In S4, the heat treatment includes: Stress relief annealing, temperature is 150-250℃, holding time is 2-4h, heating rate is 5-10℃ / min; The second stage annealing, the temperature is 300 ~ 500 ℃, the holding time is 4 ~ 24h, the heating rate is 5 ~ 10 ℃ / min; Then cool in the furnace.
9. The additive manufacturing method according to claim 4, It is characterized in that In S4, the surface treatment includes surface cleaning, surface grinding and polishing, and surface sandblasting; The surface cleaning is ultrasonic cleaning, using anhydrous ethanol as the cleaning medium, and the cleaning time is 10 to 60 minutes; The surface sandblasting uses corundum sand as the medium, and the particle size of the corundum sand is 0.5-1mm; The surface is ground and polished on #600, #1000, #2000, and #3000 sandpapers in sequence until the surface is flat and smooth.
10. A heat dissipation component, It is characterized in that The invention is prepared by using the aluminum alloy powder for additive manufacturing as claimed in any one of claims 1 to 3, or by using the additive manufacturing method as claimed in any one of claims 4 to 9.