Aluminum alloy for electric power fittings and preparation method and application of aluminum alloy
By optimizing the composition and process of aluminum alloy, high-strength, high plasticity, corrosion-resistant power metal materials were prepared, which solved the problems of high cost and performance in the existing technology that did not meet the requirements, and realized low-cost and high-performance power metal materials. , suitable for lightweight and complex environment use of power tools.
Patent Information
- Application Number
- CN202411243998.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-12
AI Technical Summary
The existing aluminum alloy for power metals cannot take into account low cost and good strength, plasticity, and corrosion resistance. In the prior art, the materials used to add expensive raw materials such as carbon nanotubes or rare earths are costly, and the performance does not meet the requirements of power metals.
By optimizing the content and proportion of aluminum alloys, including Mg, Si, Cu, Mn, Cr, Bi and other elements, and combining homogenization treatment, extrusion, forging and solid solution aging treatment processes, high strength and high plasticity are prepared. , corrosion-resistant aluminum alloy materials avoid the use of carbon nanotubes and rare earths, and reduce the cost of material preparation.
It realizes the high strength, good plasticity and corrosion resistance of power metal materials, reduces the preparation cost, can effectively replace cast iron metal tools, promotes the lightweight process of power metal tools, and is suitable for long-term use in complex environments.
Smart Images

Figure CN118932225A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electric power materials, and in particular to an aluminum alloy for electric power fittings, a preparation method thereof and applications thereof. Background Art
[0002] Power fittings are a very important part of connecting the combined power system, and refer to various metal accessories that construct the power transmission system. As an important connection fitting in the construction of the power grid, the bowl head hanging plate is mainly used to connect the suspension clamp and the insulator string, and cooperates with other accessories to connect the wires and insulation. Through the analysis of the failures of major transmission lines, it can be seen that the paralysis of the transmission lines is mainly due to the different degrees of wear and breakage of the power fittings, so the strength of the power fittings needs to be further improved. Existing power fittings mainly use cast iron or aluminum alloy composite materials. Cast iron fittings are heavy and have poor corrosion resistance; while aluminum alloy materials are light and have certain corrosion resistance, and are widely used in the field of power fittings.
[0003] Chinese patent CN 111455208 B adds carbon nanotubes to aluminum alloy in order to improve the strength of the alloy. However, carbon nanotubes do not wet aluminum liquid, making it difficult to achieve uniform distribution, and the cost is greatly increased, limiting the widespread application of this material in power fittings. Chinese patent CN202311625181.2 discloses a 6-series aluminum alloy containing rare earth and Zr, which is not only costly, but also has a tensile strength of only slightly greater than 350MPa, which does not meet the strength requirements of power fittings. Chinese patent CN202310210646.1 discloses a high-strength aluminum alloy wire and its preparation method and application. By controlling the alloy composition and preparation method, the tensile strength can reach more than 400MPa, but the elongation is less than 5%, and the material's breaking load limit and corrosion resistance and other important indicators of power fittings are not disclosed. Chinese patent CN108300907 discloses an Al-Mn-Si-Mg alloy material and a preparation method thereof, wherein an aluminum alloy is obtained by an extrusion process, but its tensile strength is only 272-316 MPa and its elongation is 7.5-11.9%, which also cannot meet the strength and plasticity requirements of electrical fittings. Summary of the invention
[0004] The main purpose of the present invention is to provide an aluminum alloy for electric power fittings, a preparation method and application thereof, so as to solve the problem in the prior art that aluminum alloy for electric power fittings cannot have both low cost and good strength, plasticity and corrosion resistance.
[0005] To achieve the above-mentioned object, according to one aspect of the present invention, there is provided an aluminum alloy for electric power fittings, comprising, by weight percentage: Mg 0.8-1.2%, Si 0.9-1.3%, Cu 0.3-1.2%, Mn 0.1-1.0%, Cr0.05-0.6%, Bi 0.01-0.05%, Ti≤0.05%, Fe≤0.5%, and the balance is Al; wherein the weight ratio of Mg to Si is (0.7-1.0):1; the weight ratio of the sum of Mn and Cr to Bi is (5-100):1.
[0006] Furthermore, in the aluminum alloy for electric power fittings, the weight ratio of Mn to Cr is (1.1-15):1, preferably (1.6-2.8):1; and / or the weight ratio of the sum of Mn and Cr to Bi is (10-55):1.
[0007] Furthermore, the aluminum alloy for electric power fittings includes, by weight percentage, Mg 0.9-1.15%, Si 0.9-1.2%, Cu 0.3-1.0%, Mn 0.2-0.8%, Cr 0.1-0.5%, Bi 0.02-0.04%, Ti≤0.02%, Fe≤0.35%, and the balance is Al.
[0008] Furthermore, the average grain size of the aluminum alloy for electric power fittings in the solid solution aging state is 6 to 12 μm, and the volume fraction of the second phase is 1 to 2.5%.
[0009] Furthermore, the yield strength of the aluminum alloy for power fittings is 380-420 MPa, and the tensile strength is 420-450 MPa; and / or the elongation of the aluminum alloy for power fittings is 11-20%; and / or the breaking load of the aluminum alloy for power fittings is 140-180 kN; and / or the mass loss of the aluminum alloy for power fittings in a salt spray atmosphere for 1000 h is ≤750 mg / cm 2 .
[0010] According to another aspect of the present invention, a method for preparing the aluminum alloy for electric power fittings of the present invention is provided, comprising the following steps: step S1, preparing materials and melting and casting according to the alloy composition to obtain an aluminum alloy ingot; step S2, homogenizing the aluminum alloy ingot to obtain a homogenized ingot; step S3, extruding the homogenized ingot to obtain an extruded material; step S4, forging the extruded material to obtain a forged material; step S5, solution aging treatment of the forged material to obtain an aluminum alloy for electric power fittings.
[0011] Further, in step S2, the temperature of the homogenization treatment is 550-570°C, the holding time is 2-12h, and the heating rate is 20-30°C / h; preferably, when the weight ratio of the sum of Mn and Cr to Bi in the aluminum alloy for power hardware is (5-40):1, the temperature of the homogenization treatment is 550-560°C, and the holding time is 9-12h; preferably, when the weight ratio of the sum of Mn and Cr to Bi in the aluminum alloy for power hardware is greater than 40:1 and less than or equal to 100:1, the temperature of the homogenization treatment is greater than 560°C and less than or equal to 570°C, and the holding time is greater than or equal to 2h and less than 9h; preferably, the area of the second phase with a diameter of ≥5μm in the homogenized ingot accounts for ≤5%.
[0012] Furthermore, in step S3, the extrusion temperature is 480-560° C., preferably 510-560° C., the extrusion ratio is 25-60, and the outlet speed is 120-180 mm / s.
[0013] Furthermore, in step S4, the forging temperature is 420-520°C; in step S5, the solution treatment temperature is 510-565°C, and the holding time is 0.5-4h; the aging treatment temperature is 160-180°C, and the holding time is 6-12h; preferably, the forging material is subjected to solution aging treatment and then surface shot peening to obtain an aluminum alloy for power fittings.
[0014] According to another aspect of the present invention, there is provided an electric power fitting, the material of which includes the aluminum alloy for electric power fittings of the present invention.
[0015] By applying the technical solution of the present invention, the content of Mg and Si in the aluminum alloy for electric power fittings is optimized, which not only ensures the high strength of the alloy, but also avoids the formation of coarse second phases due to excess Mg and Si elements; the content of Mn and Cr elements is optimized, forming a fine second phase to hinder the growth of recrystallized grains, thereby improving the grain size of the aluminum alloy for electric power fittings; the content of Cu element is optimized, so that the strength of the alloy is further improved; an appropriate amount of Bi element is added to make the aluminum alloy for electric power fittings easier to cut and process, and at the same time, the ratio of the main strengthening elements Mg and Si, as well as the ratio of the main toughening elements Mn and Cr to the characteristic element Bi of electric power fittings are limited, so as to obtain a high-strength, high-plasticity, corrosion-resistant aluminum alloy material for electric power fittings, which has good comprehensive performance, can effectively replace cast iron, and promote the lightweight process of electric power fittings. Moreover, the high-strength aluminum alloy for electric power fittings provided by the present invention does not add expensive raw materials such as carbon nanotubes and rare earths, improves the plasticity of the material and greatly reduces the material preparation cost, is easy to implement in industry, and can be widely used in electric power fittings. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0017] Figure 1 The microstructure picture of the aluminum alloy for electric power fittings after homogenization annealing according to Example 1 of the present invention is shown;
[0018] Figure 2 The 200X grain morphology of the aluminum alloy for electric power fittings in the aged state according to Example 1 of the present invention is shown; and
[0019] Figure 3 The second phase morphology of the aluminum alloy for electric power fittings in the aged state according to Example 1 of the present invention is shown. DETAILED DESCRIPTION
[0020] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0021] As described in the background of the present invention, the prior art has the problem that aluminum alloys for power fittings cannot take into account both low cost and good strength, plasticity, and corrosion resistance. In order to solve the above problem, in a typical embodiment of the present invention, an aluminum alloy for power fittings is provided, which includes, by weight percentage: Mg 0.8-1.2%, Si 0.9-1.3%, Cu0.3-1.2%, Mn 0.1-1.0%, Cr 0.05-0.6%, Bi 0.01-0.05%, Ti≤0.05%, Fe≤0.5%, and the balance is Al; wherein the weight ratio of Mg to Si is (0.7-1.0):1, and the weight ratio of the sum of Mn and Cr to Bi is (5-100):1.
[0022] Alloy composition is one of the key factors controlling the mechanical properties and corrosion resistance of materials. In the aluminum alloy for power fittings of the present invention, Mg, Si, and Cu are the main strengthening elements, forming the precursors of the strengthening phase Mg2Si or AlCuMg. However, if the content of Mg and Si is too high, on the one hand, the forming performance of the material will be reduced, and on the other hand, a large amount of residual coarse Mg2Si phase will be formed, which will significantly reduce the toughness and mechanical properties of the material; if the Cu content is too high, it is easy to form a coarse Cu-containing phase, which will reduce the corrosion resistance of the material. Therefore, the present invention controls Mg 0.8-1.2%, Si 0.9-1.3%, Cu 0.3-1.2%, and the weight ratio of Mg to Si is (0.7-1.0):1. The strengthening effect is better by the Mg, Si element content and their ratio and the Cu content within the above range, which promotes the formation of the strengthening phase and keeps the alloy strength at a high level.
[0023] Mn in the alloy mainly plays the role of inhibiting recrystallization and stabilizing subcrystalline structure, which not only improves the strength of the material but also improves the toughness, plasticity and corrosion resistance. However, too high Mn content will form too many coarse intermetallic compounds during the casting process, reducing the formability of the material. Therefore, the present invention controls Mn to 0.1-1.0%. Cr can form fine Al7(CrFe) or Al 12 CrMn phase hinders recrystallization nucleation and growth, improves alloy toughness, and reduces stress corrosion cracking sensitivity. Adding Mn and Cr elements can increase the elastic modulus and hardening index of the alloy, thereby improving the stress corrosion resistance of the alloy. In addition, AlFe (Mn, Cr) particles formed by Cr, Mn and Fe elements can enhance the wear resistance of electrical hardware; but when the Cr content is too high, it will form coarse metal compounds with other alloying elements or impurities, reducing the forming performance of the alloy. Therefore, the present invention controls Cr 0.05-0.6%.
[0024] Fe is an impurity element. When the Fe content is below 0.5%, it has little effect on the alloy properties. However, when the Fe content exceeds 0.5%, it is easy to form a coarse Fe-containing phase, which is not good for the elongation and slow stress corrosion performance of the alloy. Therefore, the present invention controls Fe≤0.5%. Ti mainly controls the cast grains. When it exceeds a certain amount (such as 0.05%), it no longer significantly affects the cast grains. Therefore, the present invention controls Ti≤0.05%.
[0025] The addition of Bi element can improve the cutting and other machining properties of the material, making the alloy suitable for electric power fittings, but Bi element is easy to form a low melting point eutectic phase, lowering the melting point of the material, and is also easy to cause overburning, thereby reducing the mechanical properties of the material. Therefore, the present invention controls Bi to 0.01-0.05%. At the same time, since electric power fittings have high requirements for the strength, toughness, corrosion resistance and other properties of aluminum alloy materials, in order to make the aluminum alloy of the present invention more suitable for use as electric power fittings, the present invention specifically limits the weight ratio of the sum of Mn and Cr to Bi to (5-100):1. By limiting the content of the above elements and Bi within a specific range, the appropriate amount of various types of intermetallic compounds can be effectively controlled, thereby providing better strength, toughness, and corrosion resistance, and meeting the long-term use requirements of electric power fittings.
[0026] In summary, the present invention optimizes the content of Mg and Si elements in the aluminum alloy for electric power fittings, which not only ensures the high strength of the alloy, but also avoids the formation of coarse second phases due to excess Mg and Si elements; optimizes the content of Mn and Cr elements, forms a fine second phase to hinder the growth of recrystallized grains, thereby improving the grain size of the aluminum alloy for electric power fittings; optimizes the content of Cu elements, so that the strength of the alloy is further improved; adds an appropriate amount of Bi element, so that the aluminum alloy for electric power fittings is easier to cut and process, and at the same time limits the ratio of the main strengthening elements Mg and Si, as well as the ratio of the main toughening elements Mn and Cr to the characteristic element Bi of electric power fittings, to obtain a high-strength, high-plasticity, corrosion-resistant aluminum alloy material for electric power fittings, with good comprehensive performance, which can effectively replace cast iron and promote the lightweight process of electric power fittings. Moreover, the high-strength aluminum alloy for electric power fittings provided by the present invention does not add expensive raw materials such as carbon nanotubes and rare earths, improves the plasticity of the material and greatly reduces the material preparation cost, is easy to implement in industry, and can be widely used in electric power fittings.
[0027] In order to achieve the best balance among the mechanical properties, corrosion resistance and cutting performance of the aluminum alloy, in a preferred embodiment, in the aluminum alloy for the electric hardware, the weight ratio of Mn to Cr is (1.1-15):1, preferably (1.6-2.8):1; and / or the weight ratio of the sum of Mn and Cr to Bi is (10-55):1. Under the above conditions, the elongation and corrosion resistance of the aluminum alloy can be further improved.
[0028] In a preferred embodiment, the aluminum alloy for power fittings includes, by weight percentage: Mg 0.9-1.15%, Si 0.9-1.2%, Cu 0.3-1.0%, Mn 0.2-0.8%, Cr 0.1-0.5%, Bi 0.02-0.04%, Ti≤0.02%, Fe≤0.35%, and the balance is Al. The aluminum alloy for power fittings within the above range can better balance strength, plasticity and corrosion resistance, and is more suitable for cutting.
[0029] In terms of microstructure, in a preferred embodiment, the average grain size of the aluminum alloy for power fittings in the solid solution aged state is 6 to 12 μm, and the volume fraction of the second phase is 1 to 2.5%. Therefore, by controlling the alloy grain size and the proportion of the second phase, the material can have higher plasticity while having good strength and corrosion resistance.
[0030] As described above, the aluminum alloy of the present invention is a high-strength, high-plasticity, corrosion-resistant aluminum alloy material for electric power fittings. Specifically, in a preferred embodiment, the yield strength of the aluminum alloy for electric power fittings is 380-420 MPa, and the tensile strength is 420-450 MPa; and / or the elongation of the aluminum alloy for electric power fittings is 11-20%; and / or the breaking load of the aluminum alloy for electric power fittings is 140-180 kN; and / or the mass loss of the aluminum alloy for electric power fittings in a salt spray atmosphere for 1000 h is ≤750 mg / cm 2 , more suitable as electrical fittings material for use in various complex environments.
[0031] In another typical embodiment of the present invention, a method for preparing the above-mentioned aluminum alloy for electric power fittings of the present invention is also provided, comprising the following steps: step S1, preparing materials and melting and casting according to the alloy composition to obtain an aluminum alloy ingot; step S2, homogenizing the aluminum alloy ingot to obtain a homogenized ingot; step S3, extruding the homogenized ingot to obtain an extruded material; step S4, forging the extruded material to obtain a forged material; step S5, solution aging treatment of the forged material to obtain an aluminum alloy for electric power fittings.
[0032] The present invention firstly prepares materials and melts the alloy components, and after the melt is refined, an aluminum alloy ingot is casted by using a semi-continuous casting device; then the aluminum alloy ingot is headed and milled, and then put into a heat treatment furnace for homogenization treatment, during which Mg2Si is dissolved, and intermetallic compounds containing Mn, Cr, and Bi are precipitated to obtain a homogenized ingot; then the homogenized ingot is extruded, during which the alloy structure is recrystallized to obtain an extruded material; then the extruded material is forged, during which the alloy structure becomes denser to obtain a forged material, and some simple electric hardware can be directly formed in this step; finally, the forged material is subjected to a solid solution aging treatment, during which a strengthening phase can be formed, so that the alloy material has a higher strength, and an aluminum alloy for electric hardware is obtained.
[0033] The present invention reasonably adjusts the total content of aluminum alloy elements such as Mg and Si and the homogenization annealing process, and controls the extrusion process and solution heat treatment, so that the main alloy elements can be dissolved into the matrix to the greatest extent, fully exerting their strengthening effect, and strictly controls the heat treatment process, so that the Fe, Mn, and Cr particles are fine and evenly dispersed in the matrix, pinning the grain boundary movement, and the grains of the extruded material are uniform and fine. Reasonable alloy composition and process ensure that the material can reach a yield strength of more than 380MPa, and has good plasticity and corrosion resistance, and better meets the use requirements of power hardware.
[0034] Specifically, in a preferred embodiment, in step S2, the temperature of the homogenization treatment is 550-570°C, the holding time is 2-12h, and the heating rate is 20-30°C / h; the weight ratio of the sum of Mn and Cr to Bi is (5-40):1, the temperature of the homogenization treatment is 550-560°C, and the holding time is 9-12h; preferably, when the weight ratio of the sum of Mn and Cr to Bi in the aluminum alloy for power fittings is greater than 40:1 and less than or equal to 100:1, the temperature of the homogenization treatment is greater than 560°C and less than or equal to 570°C, and the holding time is greater than or equal to 2h and less than 9h; preferably, the area of the second phase with a diameter of ≥5μm in the homogenized ingot accounts for ≤5%. Under the above conditions, the coarse Mg2Si phase can be more fully dissolved, and the particles containing Mn, Cr, and Bi can be more fully precipitated, which is more conducive to the further improvement of subsequent strength, toughness and corrosion resistance.
[0035] In order to better control the second phase distribution and grain size inside the aluminum alloy, thereby further improving the mechanical properties and plasticity of the aluminum alloy for power fittings, in a preferred embodiment, in step S3, the extrusion temperature is 480-560°C, preferably 510-560°C, the extrusion ratio is 25-60, and the outlet rate is 120-180 mm / s; preferably, the diameter of the extruded material is 20-50 mm, and the average grain size is 8-12 μm. Under the above conditions, especially at higher extrusion temperatures, the material grains can be further fully dynamically recrystallized, while providing higher quenching strength, providing an organizational basis for the implementation of subsequent processes.
[0036] In order to make the final state of the material have higher mechanical properties, in a preferred embodiment, in step S4, the forging temperature is 420-520°C, preferably, after the extruded material is forged, trimming and machining are performed in sequence to obtain a forged material; and / or in step S5, the temperature of the solid solution treatment is 510-565°C, and the holding time is 0.5-4h; the temperature of the aging treatment is 160-180°C, and the holding time is 6-12h; preferably, the forged material is subjected to solid solution aging treatment, and then the surface is shot peened to obtain an aluminum alloy for power fittings. Under the above conditions, the formation of the alloy strengthening phase can be further promoted, so that the strength performance of the material is further improved.
[0037] In another typical embodiment of the present invention, an electric power fitting is provided, the material of which includes the aluminum alloy for electric power fittings of the present invention, which has a low preparation cost and good strength, plasticity and corrosion resistance, and can be used for long-term stable use in complex environments.
[0038] Typically, but not limiting, the aluminum alloy for power fittings includes, by weight percentage: Mg 0.8%, 0.9%, 1.0%, 1.1%, 1.15%, 1.2% or a range consisting of any two of them, Si 0.9%, 1.0%, 1.1%, 1.2%, 1.3% or a range consisting of any two of them, Cu 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2% or a range consisting of any two of them, Mn 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0% or a range consisting of any two of them, Cr 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6% or a range consisting of any two of them, Bi 0.01%, 0.02%, 0.03%, 0.04%, 0.05% or a range consisting of any two of them, Ti≤0.05%, Fe≤0.5%, and the balance is Al.
[0039] Typically but not limiting, the weight ratio of Mg to Si is 0.7:1, 0.8:1, 0.9:1, 1.0:1 or a range consisting of any two of them.
[0040] Typically, but not limiting, the weight ratio of the sum of Mn and Cr to Bi is 5:1, 10:1, 15:1, 20:1, 30:1, 40:1, 50:1, 55:1, 60:1, 70:1, 80:1, 90:1, 100:1 or a range consisting of any two of them.
[0041] Typically, but not limitedly, the weight ratio of Mn to Cr is 1.1:1, 1.6:1, 2:1, 2.8:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1 or a range consisting of any two of them.
[0042] Typically but not limiting, in step S2, the temperature of the homogenization treatment is 550°C, 555°C, 560°C, 565°C, 570°C or a range consisting of any two of them, and the insulation time is 2h, 4h, 6h, 8h, 10h, 12h or a range consisting of any two of them.
[0043] Typically but not limitatively, when the weight ratio of the sum of Mn and Cr to Bi in the aluminum alloy for power fittings is 5:1, 10:1, 15:1, 20:1, 25:1, 30:1, 35:1, 40:1 or a range consisting of any two of them, the homogenization temperature is 550°C, 552°C, 554°C, 555°C, 556°C, 558°C, 560°C or a range consisting of any two of them, and the holding time is 9h, 10h, 11h, 12h or a range consisting of any two of them.
[0044] Typically but not limitatively, when the weight ratio of the sum of Mn and Cr to Bi in the aluminum alloy for power fittings is 41:1, 45:1, 50:1, 60:1, 70:1, 80:1, 90:1, 100:1 or a range consisting of any two of them, the homogenization temperature is 561°C, 562°C, 564°C, 565°C, 566°C, 568°C, 570°C or a range consisting of any two of them, and the holding time is 2h, 3h, 4h, 5h, 6h, 7h, 8h, 8.5h or a range consisting of any two of them.
[0045] Typically but not limiting, in step S3, the extrusion temperature is 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C or a range consisting of any two of them, and the extrusion ratio is 25, 30, 40, 50, 60 or a range consisting of any two of them.
[0046] Typically but not limiting, in step S4, the forging temperature is 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C or a range consisting of any two of them.
[0047] Typically but not limiting, in step S5, the temperature of the solution treatment is 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 565°C or a range consisting of any two of them, and the holding time is 0.5h, 1h, 2h, 3h, 4h or a range consisting of any two of them; the temperature of the aging treatment is 160°C, 165°C, 170°C, 175°C, 180°C or a range consisting of any two of them, and the holding time is 6h, 7h, 8h, 9h, 10h, 11h, 12h or a range consisting of any two of them.
[0048] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0049] Example 1
[0050] The aluminum alloy compositions are shown in Table 1.
[0051] Step S1, pure aluminum and various master alloys are melted according to the composition ratio, and the melt is refined and then cast into a round ingot of 157 mm using a semi-continuous casting device to obtain an aluminum alloy ingot;
[0052] Step S2, cutting and milling the aluminum alloy ingot, and then sending it into a heat treatment furnace, heating it to 560° C. at a rate of 25° C. / h and keeping it at that temperature for 12 hours, and then cooling it with air to obtain a homogenized ingot;
[0053] Step S3, milling the homogenized ingot, heating it to 540° C., extruding it, with an extrusion ratio of 25, an outlet speed of 150 mm / s, and water cooling to obtain an extruded rod;
[0054] Step S4, heating the extruded rod to 500° C. forging, trimming, and machining to obtain a forged material;
[0055] Step S5, subjecting the forged material to a solution treatment at 560° C. for 1 hour, quenching, aging treatment at 170° C. for 10 hours within 24 hours, and then surface shot peening to obtain an electric power fitting aluminum alloy.
[0056] Example 2
[0057] The aluminum alloy compositions are shown in Table 1.
[0058] Step S1, pure aluminum and various master alloys are melted according to the composition ratio, and the melt is refined and then cast into a round ingot of 157 mm using a semi-continuous casting device to obtain an aluminum alloy ingot;
[0059] Step S2, cutting and milling the aluminum alloy ingot, and then sending it into a heat treatment furnace, heating it to 570° C. at a rate of 30° C. / h and keeping it at that temperature for 8 hours, and then cooling it with air to obtain a homogenized ingot;
[0060] Step S3, milling the homogenized ingot, heating it to 520° C., extruding it, with an extrusion ratio of 60, an outlet speed of 160 mm / s, and water cooling to obtain an extruded rod;
[0061] Step S4, heating the extruded rod to 480° C. for forging, trimming, and machining to obtain a forged material;
[0062] Step S5, subjecting the forged material to a solution treatment at 565° C. for 0.5 h, quenching, aging treatment at 180° C. for 8 h within 24 h, and then surface shot peening to obtain an electric power fitting aluminum alloy.
[0063] Examples 3 to 12
[0064] The difference from Example 1 is that the preparation process parameters are different, see Table 2 for details.
[0065] Examples 13 to 24
[0066] The difference from Example 1 is that the aluminum alloy composition is different, see Table 1 for details.
[0067] Embodiment 25
[0068] The difference from Example 1 is that the ingredients are the same as Example 21, but the preparation process parameters are different, see Table 2 for details.
[0069] Embodiment 26
[0070] The difference from Example 1 is that the ingredients are the same as Example 1, but the preparation process parameters are different, see Table 2 for details.
[0071] Embodiment 27
[0072] The difference from Example 1 is that the ingredients are the same as Example 17, but the preparation process parameters are different, see Table 2 for details.
[0073] Embodiment 28
[0074] The difference from Example 1 is that the ingredients are the same as Example 23, but the preparation process parameters are different, see Table 2 for details.
[0075] Examples 29 to 34
[0076] The difference from Example 1 is that the preparation process parameters are different, see Table 2 for details.
[0077] Comparative Example 1
[0078] The aluminum alloy compositions are shown in Table 1.
[0079] Step S1, pure aluminum and various master alloys are melted according to the composition ratio, and the melt is refined and then cast into a round ingot of 157 mm using a semi-continuous casting device to obtain an aluminum alloy ingot;
[0080] Step S2, cutting and milling the aluminum alloy ingot, and then sending it into a heat treatment furnace, heating it to 560° C. at a rate of 30° C. / h and keeping it at that temperature for 8 hours, and then cooling it with air to obtain a homogenized ingot;
[0081] Step S3, milling the homogenized ingot, heating it to 520° C., extruding it, with an extrusion ratio of 20, an outlet speed of 160 mm / s, and water cooling to obtain an extruded rod;
[0082] Step S4, heating the extruded rod to 480° C. for forging, trimming, and machining to obtain a forged material;
[0083] Step S5, subjecting the forged material to a solution treatment at 565° C. for 0.5 h, quenching, aging treatment at 180° C. for 8 h within 24 h, and then surface shot peening to obtain an electric power fitting aluminum alloy.
[0084] Comparative Example 2
[0085] The aluminum alloy compositions are shown in Table 1.
[0086] Step S1, pure aluminum and various master alloys are melted according to the composition ratio, and the melt is refined and then cast into a round ingot of 157 mm using a semi-continuous casting device to obtain an aluminum alloy ingot;
[0087] Step S2, cutting and milling the aluminum alloy ingot, and then sending it into a heat treatment furnace, heating it to 550° C. at a rate of 30° C. / h and keeping it at that temperature for 8 hours, and then cooling it with air to obtain a homogenized ingot;
[0088] Step S3, milling the homogenized ingot, heating it to 420°C, extruding it, with an extrusion ratio of 65, an outlet speed of 160 mm / s, and water cooling to obtain an extruded rod;
[0089] Step S4, heating the extruded rod to 480° C. for forging, trimming, and machining to obtain a forged material;
[0090] Step S5, subjecting the forged material to a solution treatment at 545° C. for 0.5 h, quenching, aging treatment at 180° C. for 8 h within 24 h, and then surface shot peening to obtain an electric power fitting aluminum alloy.
[0091] Comparative Example 3
[0092] The aluminum alloy compositions are shown in Table 1.
[0093] Step S1, pure aluminum and various master alloys are melted according to the composition ratio, and the melt is refined and then cast into a round ingot of 157 mm using a semi-continuous casting device to obtain an aluminum alloy ingot;
[0094] Step S2, cutting and milling the aluminum alloy ingot, and then sending it into a heat treatment furnace, heating it to 530° C. at a rate of 30° C. / h and keeping it at that temperature for 8 hours, and then cooling it with air to obtain a homogenized ingot;
[0095] Step S3, milling the homogenized ingot, heating it to 420° C., extruding it, with an extrusion ratio of 50, an outlet speed of 160 mm / s, and water cooling to obtain an extruded rod;
[0096] Step S4, heating the extruded rod to 480° C. for forging, trimming, and machining to obtain a forged material;
[0097] Step S5, subjecting the forged material to a solution treatment at 560° C. for 5 hours, quenching, aging treatment at 160° C. for 8 hours within 24 hours, and then surface shot peening to obtain an electric power fitting aluminum alloy.
[0098] Performance Test:
[0099] The electric power fittings aluminum alloys prepared in the above examples and comparative examples were subjected to electron microscopic observation and mechanical property testing, and were prepared into electric power fittings of models WS-7 and WS-10, respectively, and the testing failure load was: GB / T 228.1-2010.
[0100] The WS-7 type electric fittings of the above-mentioned embodiment 1 and the cast iron electric fittings were subjected to corrosion resistance and Brinell hardness tests: Corrosion resistance: GB / T10125-2012 "Artificial atmosphere corrosion test salt spray test"; Brinell hardness: GB / T231-2009.
[0101] The test results are shown in Tables 3 and 4.
[0102] The microstructure of the aluminum alloy for power fittings of Example 1 after homogenization annealing is shown in Figure 1 , the 200X grain morphology of aluminum alloy aging state is shown in Figure 2 , the morphology of the second phase of aluminum alloy in aging state is shown in Figure 3 .
[0103] Depend on Figure 1 It can be seen that there are more second phases in the structure of the aluminum alloy of Example 1 after homogenization annealing, which is beneficial to the subsequent grain control and performance improvement.
[0104] Depend on Figure 2 It can be seen that the grains of the aluminum alloy in the aged state of Example 1 are fine, which is beneficial to the improvement of strength, plasticity and corrosion resistance.
[0105] Depend on Figure 3 It can be seen that there are a large number of intermetallic compounds in the aged structure of the aluminum alloy of Example 1, which is beneficial to the control of alloy grains and the increase of the breaking load.
[0106] Table 1
[0107] Weight percentage Mg Si Cu Mn Cr Bi Ti Fe Mg / Si Mn / Cr (Mn+Cr) / Bi Example 1 1 1.08 0.4 0.68 0.25 0.025 0.02 0.21 0.93 2.72 37 Example 2 0.9 1.15 1 0.8 0.1 0.03 0.02 0.18 0.78 8.00 30 Embodiment 13 0.9 0.9 0.3 1.00 2.72 37 Embodiment 14 1.15 1.2 1 0.96 2.72 37 Embodiment 15 0.2 0.1 0.93 2.00 12 Example 16 0.8 0.5 0.93 1.60 52 Embodiment 17 0.02 0.02 0.21 0.93 2.72 47 Embodiment 18 0.04 0.02 0.21 0.93 2.72 23 Embodiment 19 0.8 0.9 0.3 0.89 2.72 37 Embodiment 20 1.2 1.3 1.2 0.92 2.72 37 Embodiment 21 0.1 0.05 0.93 2.00 6 Embodiment 22 1 0.6 0.93 1.67 64 Embodiment 23 0.01 0.05 0.5 0.93 2.72 93 Embodiment 24 0.05 0.05 0.5 0.93 2.72 19 Comparative Example 1 0.6 0.8 0 0.1 0.1 0 0.02 0.18 0.75 1.00 N / A Comparative Example 2 1 0.8 0 0.1 0.1 0 0.02 0.18 1.25 1.00 N / A Comparative Example 3 0.5 1.2 0 0.1 0.1 0 0.02 0.18 0.42 1.00 N / A
[0108] "Blank" in the table refers to the same as in Example 1.
[0109] Table 2
[0110]
[0111]
[0112] "Blank" in the table refers to the same as in Example 1.
[0113] Table 3
[0114]
[0115]
[0116] Table 4
[0117]
[0118] As can be seen from the above, the aluminum alloy materials in the embodiments of the present invention have significantly better performance than existing cast iron fittings due to the control of composition, process and organization. Compared with the comparative examples, the embodiments of the present invention optimize the content of Mg and Si elements in the aluminum alloy for power fittings, which not only ensures the high strength of the alloy, but also avoids the formation of coarse second phases due to excess Mg and Si elements; optimizes the content of Mn and Cr elements, forms a fine second phase to hinder the growth of recrystallized grains, thereby improving the grain size of the aluminum alloy for power fittings; optimizes the content of Cu elements, so that the strength of the alloy is further improved; adds an appropriate amount of Bi elements, so that the aluminum alloy for power fittings is easier to cut, and at the same time limits the ratio of the main strengthening elements Mg and Si, as well as the ratio of the main toughening elements Mn and Cr to the characteristic element Bi of power fittings, to obtain a high-strength, high-plasticity, corrosion-resistant aluminum alloy material for power fittings, which has good comprehensive performance, can effectively replace cast iron, and promote the lightweight process of power fittings. Moreover, the high-strength aluminum alloy for electric power fittings provided by the present invention does not add expensive raw materials such as carbon nanotubes and rare earths, thereby improving the plasticity of the material and greatly reducing the material preparation cost. It is easy to implement in industry and can be widely used in electric power fittings.
[0119] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An aluminum alloy for electric power fittings, It is characterized in that Calculated by weight percentage, it includes: Mg 0.8-1.2%, Si 0.9-1.3%, Cu 0.3-1.2%, Mn 0.1-1.0%, Cr 0.05-0.6%, Bi 0.01-0.05%, Ti≤0.05%, Fe≤0.5%, and the balance is Al; Among them, the weight ratio of Mg to Si is (0.7-1.0):1; the weight ratio of the sum of Mn and Cr to Bi is (5-100):
1.
2. The aluminum alloy for electric power fittings according to claim 1, It is characterized in that In the aluminum alloy for electric power fittings, The weight ratio of Mn to Cr is (1.1-15):1, preferably (1.6-2.8):1; and / or The weight ratio of the sum of Mn and Cr to Bi is (10-55):
1.
3. The aluminum alloy for electric power fittings according to claim 1 or 2, It is characterized in that Calculated by weight percentage, the aluminum alloy for power fittings includes: Mg 0.9-1.15%, Si 0.9-1.2%, Cu 0.3-1.0%, Mn 0.2-0.8%, Cr0.1-0.5%, Bi 0.02-0.04%, Ti≤0.02%, Fe≤0.35%, and the balance is Al.
4. The aluminum alloy for electric power fittings according to any one of claims 1 to 3, It is characterized in that The average grain size of the aluminum alloy for electric power hardware in the solid solution aging state is 6-12 μm, and the volume fraction of the second phase is 1-2.5%.
5. The aluminum alloy for electric power fittings according to any one of claims 1 to 4, It is characterized in that The aluminum alloy for electric power fittings has a yield strength of 380-420 MPa and a tensile strength of 420-450 MPa; and / or The elongation of the aluminum alloy for electric power fittings is 11 to 20%; and / or The breaking load of the aluminum alloy for power fittings is 140-180 kN; and / or The mass loss of the aluminum alloy for power fittings in salt spray atmosphere for 1000 hours is ≤750mg / cm 2 .
6. A method for preparing the aluminum alloy for electric power fittings according to any one of claims 1 to 5, It is characterized in that The following steps are involved: Step S1, preparing materials and melting and casting according to alloy components to obtain an aluminum alloy ingot; Step S2, homogenizing the aluminum alloy ingot to obtain a homogenized ingot; Step S3, extruding the homogenized ingot to obtain an extruded material; Step S4, forging the extruded material to obtain a forged material; Step S5, subjecting the forged material to a solution aging treatment to obtain the aluminum alloy for electric power fittings.
7. The preparation method according to claim 6, It is characterized in that In step S2, the temperature of the homogenization treatment is 550-570°C, the holding time is 2-12h, and the heating rate is 20-30°C / h; Preferably, when the weight ratio of the sum of Mn and Cr to Bi in the aluminum alloy for power hardware is (5-40):1, the temperature of the homogenization treatment is 550-560° C., and the holding time is 9-12 hours; Preferably, when the weight ratio of the sum of Mn and Cr to Bi in the aluminum alloy for power hardware is greater than 40:1 and less than or equal to 100:1, the temperature of the homogenization treatment is greater than 560°C and less than or equal to 570°C, and the holding time is greater than or equal to 2h and less than 9h.
8. The preparation method according to claim 6 or 7, It is characterized in that In the step S3, the extrusion temperature is 480-560° C., preferably 510-560° C., the extrusion ratio is 25-60, and the outlet speed is 120-180 mm / s.
9. The preparation method according to any one of claims 6 to 8, It is characterized in that In the step S4, the forging temperature is 420-520°C; In the step S5, the temperature of the solution treatment is 510-565°C, and the holding time is 0.5-4h; the temperature of the aging treatment is 160-180°C, and the holding time is 6-12h; preferably, the forging material is subjected to the solution aging treatment and then the surface shot peening treatment to obtain the aluminum alloy for power fittings.
10. An electrical fitting, It is characterized in that The material of the electric power fittings comprises the aluminum alloy for electric power fittings according to any one of claims 1 to 5.