High-fluidity heat-treatment-free rare earth aluminum alloy and preparation method thereof

By adjusting the composition ratio and process flow of aluminum alloys and adding rare earth elements such as La and Ce, the problems of high melting point compounds in aluminum alloys are solved, and the high liquidity and mechanical properties are improved, which meets the needs of the High performance and low cost requirements of aluminum alloys.

CN118932230APending Publication Date: 2024-11-12SHANGHAI JIAOTONG UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411264066.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the addition of rare earth elements in the aluminum alloy leads to the formation of high melting point compounds, affecting the fluidity and cost of the alloy. In the prior art, the Er element is expensive and fails to effectively improve the overall fluidity and plasticity of the aluminum alloy.

Method used

By adjusting the composition ratio of aluminum alloy, adding high-abundance rare earth elements such as La and Ce, combining the combined action of Sr and Er, the composition and die-casting process of the alloy are optimized to prepare high-flow heat-free rare earth aluminum alloys, including Mg, Si, Mn, Sr, Ti and RE elements, and the RE elements are Ce or La, optimize the melt protection and refining process and improve the fluidity and mechanical properties of the alloy.

Benefits of technology

The high fluidity and mechanical properties of the alloy are improved, the cost of alloy preparation is reduced, the casting defects are reduced, the structural uniformity and service life of parts are improved, and the mechanical properties exceed the performance of commercial aluminum alloy T6 treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932230A_ABST
    Figure CN118932230A_ABST
Patent Text Reader

Abstract

The invention discloses a high-fluidity heat-treatment-free rare earth aluminum alloy which comprises the following components in percentage by weight: 6.5 to 7.5 percent of Mg, 2.5 to 3.5 percent of Si, 0.6 to 0.8 percent of Mn, 0.02 to 0.04 percent of Sr, 0.08 to 0.12 percent of Ti, 0.05 to 0.12 percent of RE, the RE element belongs to one of Ce and La, the total sum of other impurities is less than or equal to 0.2 percent, and the balance of Al. According to the embodiment provided by the invention, under the condition that other components are the same, the flowing property of the alloy can be obviously improved by adding a trace amount of rare earth element La, relatively high tensile strength and yield strength are kept, and the ductility is improved. The heat treatment-free rare earth aluminum alloy part prepared by the method can meet the requirements of actual production and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal materials, and in particular to a high-fluidity heat-treatment-free rare earth aluminum alloy and a preparation method thereof. Background Art

[0002] Aluminum alloys have the advantages of light weight, high strength and corrosion resistance, and are widely used in transportation, electronic communications, aerospace and many other fields. Compared with traditional deformed or cast aluminum alloys, heat-free die-cast aluminum alloys do not require subsequent treatment after die-casting to obtain parts with qualified size and shape and satisfactory organizational performance, which is of great significance to energy conservation, emission reduction, green development, achieving the "dual carbon" goal and sustainable development.

[0003] At present, Al-Mg-Si aluminum alloy is a commonly used casting aluminum alloy. It has good strength, plasticity and good corrosion resistance while improving casting fluidity. In fact, there is a mutual restriction between fluidity and room temperature mechanical properties. In response to this problem, Chinese patent CN116445773A provides a high-strength and toughness die-casting aluminum alloy and its preparation method, which improves the casting performance of the alloy while refining the eutectic silicon, primary silicon and Mg2Si formed in the modified alloy, which can achieve a significant improvement in the casting performance of the alloy. However, the silicon content of the die-casting aluminum alloy in the prior patent is relatively high, and more RE and Sr elements are required to refine and modify the eutectic silicon, primary silicon and Mg2Si phases, and the effect of refinement and modification directly affects the alloy structure performance, otherwise it will cause the strength and ductility of the aluminum alloy to decrease at the same time, thereby affecting its service life. Moreover, under the influence of genetic effects, on the one hand, the high-melting-point rare-earth-rich phase in the rare-earth intermediate alloy is difficult to melt and will be directly left inside the aluminum alloy, directly affecting the alloy properties; on the other hand, when more rare earth elements are added, it is easy to form high-melting-point rare earth compounds, which are distributed in the aluminum alloy melt in the form of fine particles, affecting the fluidity of the alloy melt. Therefore, adding more rare earth elements will lead to greater fluctuations in the alloy casting fluidity between different production batches, which is not conducive to improving the casting yield.

[0004] Fluidity reflects the flowability of liquid alloys, which is an important process performance of alloys. It determines whether the liquid alloy can fill the mold and form a casting with a complete appearance and clear contours. It also directly affects the generation of casting defects. As the temperature decreases, the casting alloy liquid changes from the pure liquid phase flow of the superheated melt to the liquid-solid two-phase mixed flow below the liquidus temperature. The pure liquid phase flowability is affected by the friction between the melt and the mold and the internal friction resistance of the melt. The internal friction resistance is proportional to the internal kinematic viscosity of the melt. The internal friction resistance increases the viscosity of the melt and the flow of the alloy is inhibited. The melt temperature and alloy composition will have a certain impact on the flowability. Therefore, under the same temperature conditions, the addition of rare earth elements can change the melt structure and density, change the viscosity, and even change the liquidus temperature. Moreover, rare earth elements can absorb a large amount of dissolved gases and form stable refractory compounds to achieve the effect of purifying the melt. They have a greater affinity with the impurity elements of the melt, and are very easy to fill the surface defects of the alloy phase in the melt, reduce the surface tension at the interface, and improve the fluidity of the melt.

[0005] The Chinese patent with publication number CN115772620A discloses a high-performance Al-Si-Mg-Mn cast aluminum alloy and a preparation method thereof. After alloying with elements such as Mg and Mn and refining AlTi5B1, and then refining and modifying with Sr and Er together, the disadvantageous factor that the deterioration of the single Sr element has a tendency to absorb gas and affects the plasticity of the alloy can be compensated, and the purpose of refining the Al matrix and the eutectic silicon structure together can be achieved. However, Er used in the prior art is an important rare earth element in the core region, and its optical properties are very outstanding. Compared with rare earth elements with higher production such as La, Ce, and Y, it is expensive. Calculated in terms of rare earth oxides, the unit price of erbium oxide is 69.9 times that of lanthanum oxide, 47.0 times that of cerium oxide, and 6.2 times that of yttrium oxide. Under the condition of the same addition amount, the alloy preparation cost is significantly increased, which is not conducive to practical application. On the other hand, the combined effect of Sr and Er provides the effect of alloy structure refinement. Sr and Er exist in the form of a large amount of high melting point compounds in the melt, which increases the proportion of the solid phase in the melt, increases the viscosity of the melt, and damages the overall fluidity of the alloy. Therefore, the overall fluidity of the alloy is not improved, and the overall plasticity of the alloy is insufficient. In view of the above problems, the present invention adjusts the composition ratio of the base alloy, adds high-abundance rare earth elements such as La and Ce, reduces the alloy preparation cost, improves the alloy mechanical properties and fluidity, and develops a high-fluidity heat-treatment-free rare earth aluminum alloy. Summary of the invention

[0006] In view of the deficiencies in the prior art, the present invention provides a high-fluidity heat-treatment-free rare earth aluminum alloy and a preparation method thereof.

[0007] The present invention is achieved through the following technical solutions:

[0008] The present invention provides a high-fluidity heat-treatment-free rare earth aluminum alloy, which is prepared from raw materials including the following components by weight percentage:

[0009] Mg: 6.5-7.5wt.%, Si: 2.5-3.5wt.%, Mn: 0.6-0.8wt.%, Sr: 0.02-0.04wt.%, Ti: 0.08-0.12wt.%, RE: 0.05-0.12wt.%, the balance is Al and unavoidable impurity elements;

[0010] The RE element includes one of Ce and La, and the content of the impurity element is less than or equal to 0.2 wt.%.

[0011] The present invention also provides a method for preparing the high-fluidity heat-treatment-free rare earth aluminum alloy, comprising the following steps:

[0012] S1. Raw material preheating: preheating industrial pure aluminum, industrial pure magnesium, aluminum silicon master alloy, aluminum manganese master alloy, aluminum titanium master alloy, aluminum strontium master alloy, aluminum rare earth master alloy raw materials;

[0013] S2. Alloy smelting: Melt the preheated raw materials, perform melt protection, adjust the temperature, and refine to obtain a pure aluminum alloy melt;

[0014] S3. Die casting: The aluminum alloy melt is die-casted to obtain an aluminum alloy sample.

[0015] Preferably, before step S1, the process also includes blending industrial pure aluminum, industrial pure magnesium, aluminum silicon master alloy, aluminum manganese master alloy, aluminum titanium master alloy, aluminum strontium master alloy, and aluminum rare earth master alloy according to the components of the rare earth aluminum alloy and their mass percentages.

[0016] Preferably, the aluminum rare earth master alloy includes at least one of an aluminum cerium master alloy and an aluminum lanthanum master alloy.

[0017] Preferably, the preheating temperature in step S1 is 150-200° C., and the preheating time is 2-3 hours.

[0018] Preferably, the melting method in step S2 comprises: after melting industrial pure aluminum to obtain a melt, raising the melt temperature to 760-780°C, adding preheated aluminum-silicon master alloy and aluminum-manganese master alloy, adjusting the melt temperature to 680-700°C after complete melting, adding preheated industrial pure magnesium, aluminum-titanium master alloy, aluminum-strontium master alloy, and aluminum-rare earth master alloy, and pressing them below the liquid surface.

[0019] Preferably, the melt protection method in step S2 includes gas protection, and the gas is a CO2 / SF6 mixed gas.

[0020] In some embodiments, the volume ratio of CO2 to SF6 is about 1:2.

[0021] Preferably, the method for adjusting the temperature in step S2 includes adjusting the temperature to 740-760°C.

[0022] Preferably, the refining method in step S2 comprises adding an aluminum-magnesium alloy refining agent, stirring, standing at 720-740° C. for 15-20 min, and skimming off scum.

[0023] Preferably, the refining agent can remove impurities from the alloy melt and reduce metal loss.

[0024] Preferably, the amount of the refining agent added is 3-5% of the mass of the raw material.

[0025] Preferably, the die-casting method in step S3 includes: a pouring temperature of 700-720°C, a low speed of 0.2-0.4 m / s, a fast speed of 3-5 m / s, a boost pressure of 60-100 MPa, a mold retention time of 10-20s, and a mold preheating temperature of 260-280°C.

[0026] If rare earth elements are added excessively or improperly, coarse rare earth compounds with high melting points are easily formed, which significantly increase the solid phase percentage of the alloy melt, increase the melt viscosity and thus affect the fluidity of the alloy. Correspondingly, the organizational composition of the rare earth master alloy will also bring similar results, and only a specific addition amount can achieve the comprehensive performance of the present invention.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The alloy of the present invention has a greater affinity for rare earth elements with hydrogen, oxygen, nitrogen, sulfur and other impurity elements in the alloy melt, and can absorb a large amount of dissolved gas to form a stable refractory compound, which is discharged in the form of slag. In addition, the relatively active rare earth atoms in the melt can easily fill the surface defects of the alloy phase, reduce the surface tension at the interface, thereby improving the fluidity of the alloy, and the melt can smoothly fill the mold cavity to obtain parts with uniform and stable microstructure, thereby reducing the occurrence of casting defects;

[0029] (2) The rare earth aluminum alloy of the present invention is suitable for die casting, and can provide a faster cooling rate than gravity casting, making the alloy structure fine and uniform. At the same time, the rare earth-rich phase in the alloy can exist as a reinforcing phase, improving the mechanical properties under the action of multiple effects. The test results show that the mechanical properties of the rare earth aluminum alloy of the present invention exceed those of the commercial aluminum alloy after T6 treatment;

[0030] (3) Cast aluminum alloys need to undergo multiple processes such as deformation processing and heat treatment to achieve corresponding performance. However, the alloy of the present invention is used directly in a die-cast state. The high performance of the cast alloy is achieved by adjusting the alloy composition ratio, optimizing the die-casting process, etc., and further heat treatment is avoided. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0032] Figure 1 are microstructure photographs of Examples 1-3 of the present invention and Comparative Example 9, wherein a is a microstructure photograph of Example 1, b is a microstructure photograph of Example 2, c is a microstructure photograph of Example 3, and d is a microstructure photograph of Comparative Example 9;

[0033] Figure 2 The fluidity test results of Examples 1-3 of the present invention and Comparative Example 9, wherein a is the fluidity test result of Example 1, b is the fluidity test result of Example 2, c is the fluidity test result of Example 3, and d is the fluidity test result of Comparative Example 9. DETAILED DESCRIPTION

[0034] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0035] Examples 1-3

[0036] Examples 1-3 respectively provide a high-fluidity heat-treatment-free rare earth aluminum alloy, the composition of which is shown in Table 1; the preparation method comprises the following steps:

[0037] Step (1), raw material proportioning: industrial pure aluminum, industrial pure magnesium, aluminum silicon 10 master alloy, aluminum manganese 10 master alloy, aluminum titanium 10 master alloy, aluminum strontium 10 master alloy, aluminum cerium 30 master alloy are proportioned according to the components of the aluminum alloy and their mass percentages;

[0038] Step (2), preheating the raw materials: preheat the above industrial pure aluminum, industrial pure magnesium, aluminum silicon 10 master alloy, aluminum manganese 10 master alloy, aluminum titanium 10 master alloy, aluminum strontium 10 master alloy, and aluminum cerium 30 master alloy raw materials at 200° C. for 3 hours.

[0039] Step (3), alloy smelting: After preheating industrial pure aluminum in a crucible, adjust the melt temperature to 780°C, add preheated aluminum silicon 10 master alloy and aluminum manganese 10 master alloy until completely melted, adjust the melt temperature to 700°C, add preheated industrial pure magnesium, aluminum titanium 10 master alloy, aluminum strontium 10 master alloy, aluminum rare earth master alloy, and use a bell jar to press it below the liquid surface to prevent element burnout. Adjust the melt temperature to 740°C, add aluminum-magnesium alloy refining agent (commercially available casting aluminum alloy smelting flux, purchased from Henan Jingkang Industrial Co., Ltd.) to the alloy melt, the addition amount is 5% of the total mass of all raw materials, the refining agent can remove impurities in the alloy melt and reduce metal loss. After fully stirring, let it stand for refining, stand at 720°C for 20 minutes, and skim off the scum. The alloy smelting process adopts gas protection, and the protective atmosphere is a CO2 / SF6 mixed gas with a volume ratio of 1:2.

[0040] Step (4), die casting: The obtained alloy melt was die-casted at 700°C using a LK 900T cold chamber die casting machine, IMPRESS-PLUSDCC130-900, LK Group. The die casting process parameters were low speed of 0.4 m / s, fast speed of 4 m / s, boost pressure of 100 MPa, mold retention time of 10 s, and mold preheating temperature of 270°C to obtain an aluminum alloy sample.

[0041] Comparative Examples 1 and 2

[0042] Comparative Examples 1 and 2 respectively provide a high-fluidity heat-treatment-free rare earth aluminum alloy, the composition of which is shown in Table 1; the preparation method is the same as that of Example 1.

[0043] Comparative Examples 3-8

[0044] The difference between Comparative Examples 3-8 and Example 1 is that the alloy composition ratios are different.

[0045] Comparative Example 9

[0046] The difference between Comparative Example 9 and Example 1 is that no rare earth element is added.

[0047] Comparative Example 10

[0048] The difference between Comparative Example 10 and Example 1 is that the Mg content is 1 wt %.

[0049] Comparative Example 11

[0050] The only difference between Comparative Example 11 and Example 1 is that the Si content is 5 wt %.

[0051] The weight percentages of the components in the embodiments and comparative examples are shown in Table 1.

[0052] Table 1 Weight percentage of each component except aluminum and impurity elements in each embodiment and comparative example

[0053]

[0054]

[0055] Performance Testing

[0056] 1. Room temperature mechanical properties

[0057] The aluminum alloy obtained by die casting is subjected to room temperature tensile test in accordance with the requirements of GB / T 228.1-2021 "Tensile test of metallic materials Part 1: Room temperature test method" to test the room temperature mechanical properties of the alloy, including tensile strength, yield strength and elongation.

[0058] 2. Liquidity

[0059] The rare earth aluminum alloy was tested for fluidity in a triple helix alloy fluidity tester, using the concentric triple helix alloy fluidity tester and operating method described in Chinese patent CN88204038U.

[0060] 3. Microstructure

[0061] The sample surface was observed after conventional abrasion and erosion treatment using a VEGA 3 lanthanum hexaboride scanning electron microscope.

[0062] Figure 1 The microstructure photos of Examples 1-3 and Comparative Example 9 of the present invention, wherein a is the microstructure photo of Example 1, b is the microstructure photo of Example 2, c is the microstructure photo of Example 3, and d is the microstructure photo of Comparative Example 9. Figure 1 It can be seen that compared with the alloy without adding high-abundance rare earth elements La, Ce, and Y, the rare earth aluminum alloy provided by the present invention adds 0.1wt.% of high-abundance rare earth elements La, Ce, and Y, and the Al matrix and eutectic silicon structure of the alloy are both refined. Moreover, by comparing different rare earth elements, it can be seen that the rare earth element La has a better effect on matrix refinement.

[0063] The performance test results of room temperature mechanical properties and fluidity are shown in Table 2.

[0064] Table 2 Performance test results

[0065]

[0066] Figure 2The fluidity test results of Examples 1-3 of the present invention and Comparative Example 9, wherein a is the fluidity test result of Example 1, b is the fluidity test result of Example 2, c is the fluidity test result of Example 3, and d is the fluidity test result of Comparative Example 9. The better the fluidity, the longer the spiral line. The spiral line of Figure d is obviously shorter than that of Figures ac. Figure 2 It can be seen that for different rare earth elements, the rare earth Ce and La content can improve the alloy fluidity within a certain range, and too high a content will damage the overall fluidity, while the addition of rare earth Y is not conducive to improving the alloy fluidity, and further increase will obviously damage the alloy fluidity. From the perspective of mechanical properties, there are differences in the effects of different rare earth elements on alloy properties. The effect of the Y element on tensile strength is lower than that of Ce and La, and the effect of the Ce element on elongation is higher than that of La and Y. In particular, in Example 2, when other components are the same, adding a trace amount of the rare earth element La can significantly improve the alloy fluidity, while maintaining a high tensile strength and yield strength, and the elongation is improved. Therefore, the embodiment provided by the present invention has good fluidity and room temperature mechanical properties.

[0067] In summary, the present invention discloses a high-fluidity heat-treatment-free rare earth aluminum alloy, which includes components calculated by weight percentage: Mg content is 6.5-7.5wt.%, Si content is 2.5-3.5wt.%, Mn content is 0.6-0.8wt.%, Sr content is 0.02-0.04wt.%, Ti content is 0.08-0.12wt, RE content is 0.05-0.12wt.%, and the RE element is one of Ce, La, and Y. The total amount of other impurities is less than or equal to 0.2wt.%, and the balance is Al. In the embodiment provided by the present invention, when other components are the same, adding a trace amount of rare earth element La can significantly improve the fluidity of the alloy, maintain a high tensile strength and yield strength, and improve the elongation. The method of the present invention is used to prepare heat-treatment-free rare earth aluminum alloy parts, which can meet the actual production and mechanical performance requirements.

[0068] It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various changes or modifications within the scope of the claims, which do not affect the essence of the present invention. In the absence of conflict, the embodiments of the present application and the features in the embodiments may be combined with each other at will.

Claims

1. A high-fluidity heat-treatment-free rare earth aluminum alloy, characterized in that: The raw materials are prepared from the following components by weight percentage: Mg: 6.5-7.5wt.%, Si: 2.5-3.5wt.%, Mn: 0.6-0.8wt.%, Sr: 0.02-0.04wt.%, Ti: 0.08-0.12wt.%, RE: 0.05-0.12wt.%, the balance is Al and unavoidable impurity elements; The RE element includes one of Ce and La, and the content of the impurity element is less than or equal to 0.2 wt.%.

2. A method for preparing a rare earth aluminum alloy according to claim 1, characterized in that: The following steps are involved: S1. Raw material preheating: preheating industrial pure aluminum, industrial pure magnesium, aluminum silicon master alloy, aluminum manganese master alloy, aluminum titanium master alloy, aluminum strontium master alloy, aluminum rare earth master alloy raw materials; S2. Alloy smelting: Melt the preheated raw materials, perform melt protection, adjust the temperature, and refine to obtain a pure aluminum alloy melt; S3. Die casting: The aluminum alloy melt is die-casted to obtain an aluminum alloy sample.

3. The preparation method according to claim 2, characterized in that: The aluminum rare earth master alloy includes at least one of an aluminum cerium master alloy and an aluminum lanthanum master alloy.

4. The preparation method according to claim 2, characterized in that: The preheating temperature in step S1 is 150-200° C., and the preheating time is 2-3 hours.

5. The preparation method according to claim 2, characterized in that: The melting method described in step S2 includes: after melting industrial pure aluminum to obtain a melt, raising the melt temperature to 760-780°C, adding preheated aluminum-silicon master alloy and aluminum-manganese master alloy, adjusting the melt temperature to 680-700°C after complete melting, adding preheated industrial pure magnesium, aluminum-titanium master alloy, aluminum-strontium master alloy, and aluminum-rare earth master alloy, and pressing them below the liquid surface.

6. The preparation method according to claim 2, characterized in that: The melt protection method in step S2 includes gas protection, and the gas is a CO2 / SF6 mixed gas.

7. The preparation method according to claim 2, characterized in that: The method for adjusting the temperature in step S2 includes adjusting the temperature to 740-760°C.

8. The preparation method according to claim 2, characterized in that: The refining method in step S2 includes adding an aluminum-magnesium alloy refining agent, stirring, standing at 720-740° C. for 15-20 minutes, and skimming off scum.

9. The preparation method according to claim 8, characterized in that: The amount of the refining agent added is 3-5% of the mass of the raw material.

10. The preparation method according to claim 2, characterized in that: The die-casting method in step S3 includes: a pouring temperature of 700-720°C, a low speed of 0.2-0.4m / s, a fast speed of 3-5m / s, a boost pressure of 60-100MPa, a mold retention time of 10-20s, and a mold preheating temperature of 260-280°C.

Citation Information

Cited By

  • Die-casting heat-treatment-free alloy synergistically reinforced by multiple rare earth elements and preparation method thereof

    CN121575279A