Aall-d Heusler alloy capable of greatly increasing martensite phase transformation temperature and preparation method and application of all-d Heusler alloy

By introducing high melting point metals Zr, Nb, Hf, Ta, Mo, W into Ni-Co-Mn-Ti alloy, the all-d Heusler alloy was prepared, and the problem of limited temperature range of Ni-Mn-based alloy was solved, and the problem of achieving the Efficient magneto-thermal effect and a wide range of magnetic device applications.

CN118932235APending Publication Date: 2024-11-12国瑞科创稀土功能材料(赣州)有限公司 +1

Patent Information

Application Number
CN202410990984.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing Ni-Mn-based Heusler alloy has a limited magnetic-thermal effect operating temperature in different temperature ranges, and no high melting point transition metal is introduced for magnetic phase transition regulation, which limits its application potential.

Method used

The 4d and 5d transition group high melting point metals Zr, Nb, Hf, Ta, Mo, W were introduced into the Ni-Co-Mn-Ti alloy, and the all-d Heusler alloy was prepared by high vacuum smelting and rapid solidification technology to adjust the magnetization and The phase change temperature realizes the magnetic inverse martensite phase transformation driven by magnetic field.

Benefits of technology

It significantly improves the martensite phase transition temperature and widens the refrigeration temperature zone. The alloy has high strength, hardness, corrosion resistance and good magnetic field-driven variable magnetic inverse martensite phase transition characteristics, and is suitable for a variety of magnetic devices and solid state refrigeration. Device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932235A_ABST
    Figure CN118932235A_ABST
Patent Text Reader

Abstract

The invention provides an all-dHeusler alloy capable of greatly increasing the martensite phase transformation temperature and a preparation method and application thereof, the chemical formula of the all-dHeusler alloy is Ni37Co13Mn35Ti15-xTx, x is larger than or equal to 0 and smaller than or equal to 15, x represents the atomic percent content, and T is any one of 4d and 5d transition group high-melting-point metal of Zr, Nb, Hf, Ta, Mo and W. The invention further provides a preparation method of the all-d Heusler alloy capable of greatly increasing the martensite phase transformation temperature. According to the preparation method, any one of Zr, Nb, Hf, Ta, Mo and W is doped into the Ni-Co-Mn-Ti alloy through high-vacuum melting, and the all-d Heusler alloy capable of keeping the excellent magnetothermal effect and greatly widening the refrigeration temperature zone at the same time is prepared. The alloy plays a crucial role in promoting the room-temperature and high-temperature application of solid-state refrigeration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an all-d Heusler alloy material capable of greatly improving the martensitic phase transition temperature, a preparation method and application thereof, and in particular to an all-d Heusler alloy capable of greatly improving the martensitic phase transition temperature, a preparation method and application thereof. Background Art

[0002] In recent years, all-dHeusler alloys, which replace the pd orbital hybridization of Heusler alloys with dd orbital hybridization between transition metals, have become a new type of ferromagnetic martensitic phase transition system with rich physical states. Its multifunctional properties can be widely used in magnetic storage, solid-state refrigeration devices, magnetic drives, magnetic sensitive elements, magnetic heat pumps, thermal magnetoelectric conversion and other fields. The new all-transition metal Ni-Co-Mn-Ti based magnetic Heusler alloy has an adjustable giant magnetocaloric effect and good mechanical properties. Due to the inherent thermal hysteresis ΔT of the first-order phase transition hys It will lead to the irreversible characteristics of magnetic field-induced reverse martensite. Obtaining a large reversible magnetocaloric effect during magnetic field cycling is still one of the challenges for the magnetic refrigeration application of Ni-Co-Mn-Ti alloy. At present, in Ni-Mn-based alloys, the magnetocaloric effect and phase transition temperature are regulated by replacing Ni or Mn elements. Shengwei Li et al. obtained an adjustable phase transition temperature by changing the composition of Ni-Mn-Ti, and added B to improve the mechanical properties. Similarly, in Ni-Co-Mn-Ti, interstitial doping of B reduced thermal hysteresis and improved the magnetocaloric effect. In addition, the doping of Pd and Pt also affects the martensitic phase transformation of Ni-Mn-Sn. The substitution of Fe at different atomic positions (Ni or Mn positions) can adjust Ni due to changes in the concentration of valence electrons. 50 Mn 35 In 15The martensitic phase transition temperature and magnetic properties of Ni-Co-Mn-In alloys are controlled by replacing In with a small amount of Si. In addition, due to the narrow phase transition region, the operating temperature range of the magnetocaloric effect in these alloys is usually limited to a limited scale, which also imposes a strong constraint on the operating temperature range of refrigeration applications. Therefore, exploring and studying new magnetic materials with large magnetocaloric effects in different temperature ranges is a hot topic in applied physics today. In this way, it is extremely important to be able to control the martensitic phase transition Ni-Mn-based Heusler alloy with a wide refrigeration temperature range. It is worth noting that no one has ever introduced high-melting point transition metals into Ni-Mn-based Heusler alloys for magnetic phase transition research. Metals such as Zr, Nb, Hf, Ta, Mo, and W have excellent chemical stability and strong corrosion resistance due to their high melting points. Therefore, it is of great research significance to introduce any of the high-melting point metals of the 4d and 5d transition groups, such as Zr, Nb, Hf, Ta, Mo, and W, into Ni-Mn-based Heusler alloys to control the phase transition. Summary of the invention

[0003] In view of the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide an all-d Heusler alloy that can significantly increase the martensitic phase transition temperature, and a preparation method and application thereof. The all-d Heusler alloy is an alloy material with adjustable phase transition temperature. The preparation method of the material is to dope any one of Zr, Nb, Hf, Ta, Mo, and W in the 4d and 5d transition family high melting point metals into a Ni-Co-Mn-Ti alloy by high vacuum melting, and then prepare an all-d Heusler alloy that can maintain excellent magnetocaloric effect and significantly broaden the refrigeration temperature range by rapid solidification.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0005] The first object of the present invention is to provide an all-d Heusler alloy capable of significantly increasing the martensitic phase transition temperature. The chemical formula of the all-d Heusler alloy capable of significantly increasing the martensitic phase transition temperature is Ni 37 Co 13 Mn 35 Ti 15- x T x , wherein 0≤x≤15, x represents the atomic percentage content, T is a 4d or 5d transition group high melting point metal, and the 4d or 5d transition group high melting point metal is any one of Zr, Nb, Hf, Ta, Mo, and W.

[0006] Preferably, when the introduced transition metal with high melting point is Zr, the chemical formula of the alloy is Ni37 Co 13 Mn 35 Ti 15-x Zr x , where 0≤x≤15; or

[0007] When the introduced transition metal with high melting point is Nb, the chemical formula of the alloy is Ni 37 Co 13 Mn 35 Ti 15-x Nb x , where 0≤x≤15; or

[0008] When the introduced transition metal with high melting point is Hf, the chemical formula of the alloy is Ni 37 Co 13 Mn 35 Ti 15-x Hf x , where 0≤x≤15; or

[0009] When the introduced transition metal with high melting point is Ta, the chemical formula of the alloy is Ni 37 Co 13 Mn 35 Ti 15-x Ta x , where 0≤x≤15; or

[0010] When the introduced transition metal with high melting point is Mo, the chemical formula of the alloy is Ni 37 Co 13 Mn 35 Ti 15-x Mo x , where 0≤x≤15 or

[0011] When the introduced transition metal with high melting point is W, the chemical formula of the alloy is Ni 37 Co 13 Mn 35 Ti 15-x W x , where 0≤x≤15.

[0012] The second purpose of the present invention is to introduce any one of the 4d, 5d transition group high melting point metals of Zr, Nb, Hf, Ta, Mo, and W into the Ni-Co-Mn-Ti Heusler alloy, so that the alloy is doped with the 4d, 5d transition group high melting point metals so that the introduced metal forms new covalent bonds to adjust the magnetization intensity of the alloy and the sensitivity of the martensitic phase transformation to the magnetic field, and realize the magnetic field-driven variable magnetism reverse martensitic phase transformation while the temperature-driven martensitic phase transformation occurs.

[0013] The present invention provides a method for preparing an all-d Heusler alloy capable of significantly increasing the martensitic phase transition temperature, comprising the following steps:

[0014] Calculate the mass of any one 4d or 5d transition group high melting point metal element of Ni, Co, Mn, Ti, Zr, Nb, Hf, Ta, Mo, or W required according to the stoichiometric ratio, and prepare the ingredients;

[0015] Arc melting was used to obtain alloy ingot samples;

[0016] The surface of some alloy ingot samples obtained above was polished, placed in a quartz tube with an opening diameter of 1 mm at one end, and placed in a high vacuum belt spinning device. The vacuum degree was drawn to 8×10 -4 Pa, argon is filled into the belt-spinning furnace to make the internal pressure reach -0.05MPa, and the external argon pressure is adjusted to 0.05MPa, so that there is a pressure difference of 0.1MPa inside and outside the quartz tube;

[0017] The rotation speed of the copper roller and the heating current of the induction coil are adjusted, and the molten alloy is sprayed onto the rotating copper roller by using the air pressure difference to quickly solidify and form a fast-quenching strip with uniform composition and structure.

[0018] Preferably, the doping amount of any one 4d, 5d transition group high melting point metal element of Zr, Nb, Hf, Ta, Mo, and W is 1 at.%-15 at.%.

[0019] Preferably, the mass of any one 4d, 5d transition group high melting point metal element among Ni, Co, Mn, Ti, Zr, Nb, Hf, Ta, Mo, and W needs to be accurate to two decimal places in milligrams, and the purity of the element needs to be controlled at more than 99.99%.

[0020] Preferably, during the arc melting, the raw materials are placed in a water-cooled copper crucible arc furnace, 0.03 Pa of argon gas is filled into the furnace for gas washing, and then the vacuum degree is drawn to 5×10 -3 Pa, fill with 0.7 atmospheres of argon gas with a purity of 99.999% for arc melting;

[0021] For the first smelting, use 50A-70A current to melt the metal. When the metal in the crucible flows in liquid state, the first smelting is completed and turned over. Increase the current to 100A-105A and smelt 4 more times to obtain the alloy ingot.

[0022] Preferably, the molten alloy is sprayed onto a rotating copper roller by using air pressure difference to quickly solidify and form a quick-quenching strip. The copper roller speed and induction coil heating current conditions are as follows: the copper roller speed is 15m / s, and when the induction coil heating current reaches 35A or more, the alloy ingot is observed to turn red. The current is further increased to 40A or more until the alloy ingot flows in liquid state.

[0023] The third purpose of the present invention is to provide an all-dHeusler alloy that can significantly increase the martensitic phase transition temperature for use in the preparation of magnetic storage devices, magnetic drives, temperature sensitive elements, magnetic sensitive elements, magnetic heat pumps, magnetic sensors, thermomagnetic electric conversion devices and solid-state refrigeration devices.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. Ni provided by the present invention 37 Co 13 Mn 35 Ti 15-x T x In addition to the properties of common magnetic phase change materials, such as temperature or pressure (internal pressure or external pressure) can cause the material to undergo a martensitic phase transition between a weak magnetic martensite phase and a strong magnetic austenite phase. In this alloy, the magnetic field can also drive the reverse martensitic phase transition from the weak magnetic martensite phase to the strong magnetic austenite parent phase. In particular, this material has a higher phase transition temperature than the previously discovered Heusler alloys, which makes the alloy have a wider application temperature range.

[0026] 2. The Ni in the method for significantly increasing the phase transition temperature of all-d Heusler alloy provided by the present invention 37 Co 13 Mn 35 Ti 15-x T x Heusler alloys have high strength, high hardness, corrosion resistance, good mechanical properties and magnetic field driven reverse martensitic transformation. Physical parameters such as strength, hardness, martensitic transformation temperature and reverse martensitic transformation temperature, and magnetization intensity of martensite and austenite main phases can be adjusted by changing the composition of each component in the alloy.

[0027] 3. Ni provided by the present invention 37 Co 13 Mn 35 Ti 15-x T x Heusler alloys have multifunctional properties near the magnetic field driven variable magnetism reverse martensitic phase transition, including magneto-strain effect, magnetoresistance effect and magnetocaloric effect. 37 Co 13Mn 35 Ti 15-x T x Heusler alloys can be widely used in the preparation of magnetic storage, magnetic drives, temperature sensitive elements, magnetic sensitive elements, magnetic heat pumps, magnetic sensors, thermomagnetic electric conversion devices and solid-state refrigeration devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The isofield thermal magnetic curve of the alloy provided in Example 1 of the present invention;

[0029] Figure 2 The isothermal magnetization curve of the alloy provided in Example 1 of the present invention;

[0030] Figure 3 The magnetic entropy change curve of the alloy provided in Example 1 of the present invention;

[0031] Figure 4 The isofield thermal magnetic curve of the alloy provided in Example 2 of the present invention;

[0032] Figure 5 The isothermal magnetization curve of the alloy provided in Example 2 of the present invention;

[0033] Figure 6 The magnetic entropy change curve of the alloy provided in Example 2 of the present invention;

[0034] Figure 7 The isofield thermomagnetic curve of the alloy provided in Example 3 of the present invention;

[0035] Figure 8 The isofield thermal magnetic curve of the alloy provided in Example 4 of the present invention;

[0036] Fig. 9 The isofield thermal magnetic curve of the alloy provided in Example 5 of the present invention;

[0037] Fig.10 The isothermal magnetization curve of the alloy provided in Example 5 of the present invention;

[0038] Fig.11 The magnetic entropy change curve of the alloy provided in Example 5 of the present invention;

[0039] Fig.12 The isofield thermal magnetic curve of the alloy provided in Example 6 of the present invention;

[0040] Fig.13 The isofield thermomagnetic curve of the alloy provided in Example 7 of the present invention;

[0041] Fig.14 The isofield thermal magnetic curve of the alloy provided in Example 8 of the present invention;

[0042] Fig.15 The isofield thermomagnetic curve of the alloy provided in Example 9 of the present invention;

[0043] Fig.16 The isofield thermomagnetic curve of the alloy provided in Example 10 of the present invention;

[0044] Fig.17 These are the equifield thermal magnetic curves of the alloys provided in Examples 1, 2, 5 and 11 of the present invention. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any numerical value between the two endpoints can be selected. Since the steps and methods used are the same as those in Examples 1-10, in order to avoid redundancy, the present invention describes a preferred embodiment, but the present invention is not limited thereto, but can also be specifically implemented in other ways within the scope of the technical solution defined in the attached claims.

[0047] The chemical formula of the all-d Heusler alloy that can significantly increase the martensitic transformation temperature is Ni 37 Co 13 Mn 35 Ti 15-x T x , wherein 0≤x≤15, x represents the atomic percentage content, T is a 4d or 5d transition group high melting point metal, and the 4d or 5d transition group high melting point metal is any one of Zr, Nb, Hf, Ta, Mo, and W.

[0048] That is, by introducing any 4d, 5d transition group high melting point metal of Zr, Nb, Hf, Ta, Mo, W into Ni-Co-Mn-Ti Heusler alloy, the alloy is doped with 4d, 5d transition group high melting point metal, so that the introduced metal forms a new covalent bond to adjust the magnetization intensity of the alloy and the sensitivity of the martensitic phase transition to the magnetic field, and realize the magnetic field driven reverse martensitic phase transition while the temperature driven martensitic phase transition occurs. At the same time, the corresponding strip sample or alloy block sample is made to obtain the ideal primary magnetic structure phase transition and its corresponding magnetostrictive effect (magnetocaloric effect, magnetoresistance effect, magnetostrictive strain).

[0049] Based on the above principles, there are actually at least six alloy expressions:

[0050] The first chemical formula of the alloy is composed of five metal elements: Ni, Co, Mn, Ti, and Zr. Specifically, Ni 37 Co 13 Mn 35 Ti 15-x Zr x (0≤x≤15).

[0051] The second general chemical formula of the alloy is composed of five metal elements: Ni, Co, Mn, Ti, and Nb. Specifically, Ni 37 Co 13 Mn 35 Ti 15-x Nb x (0≤x≤15).

[0052] The third general chemical formula of the alloy consists of five metal elements: Ni, Co, Mn, Ti, and Hf. Specifically, Ni 37 Co 13 Mn 35 Ti 15-x Hf x (0≤x≤15).

[0053] The fourth general chemical formula of the alloy is composed of five metal elements: Ni, Co, Mn, Ti, and Ta. Specifically, Ni 37 Co 13 Mn 35 Ti 15-x Ta x (0≤x≤15).

[0054] The fifth chemical formula of the alloy is composed of five metal elements: Ni, Co, Mn, Ti, and Mo. Specifically, Ni 37 Co 13 Mn 35 Ti 15-x Mo x (0≤x≤15).

[0055] The sixth chemical formula of the alloy is composed of five metal elements: Ni, Co, Mn, Ti, and W. Specifically, Ni 37 Co 13 Mn 35 Ti 15-x W x (0≤x≤15).

[0056] The technical solution of the present invention is further illustrated below in the form of specific examples.

[0057] Example 1

[0058] Example 1 is a third alloy satisfying the general chemical formula Ni 37 Co 13 Mn 35 Ti 15-x Hf x , Hf doping amount is 1at.%, that is, the alloy Ni with martensitic phase transformation 37 Co 13 Mn 35 Ti 14 Hf1.

[0059] The present embodiment 1 is a method for preparing an all-d Heusler alloy having a martensitic phase transition temperature by adding Hf into Ni-Co-Mn-Ti, comprising the following steps:

[0060] The required mass of Ni, Co, Mn, Ti and Hf elements is calculated according to the stoichiometric ratio and the ingredients are prepared with an accuracy of 0.1mg-0.01mg. The purity of the metal elements is above 99.99%.

[0061] The prepared raw materials are placed in a water-cooled copper crucible arc melting furnace and the vacuum degree is drawn to 5×10 -3 Pa, fill with argon gas with a purity of 99.999% at 0.7 atmospheres, and perform arc melting. In the first melting, use 50A current to melt the metal. When the metal liquid in the crucible flows, turn over the block sample from the first melting, then increase the current to 100A-105A and melt it for another 4 times to get Ni 37 Co 13 Mn 35 Ti 14 Hf1 alloy ingot;

[0062] The surface of some alloy ingot samples was polished, placed in a quartz tube with an opening diameter of 1 mm at one end, and placed in a high vacuum belt spinning device. The vacuum degree was drawn to 8×10 -4 Pa, argon is filled into the belt-spinning furnace to make the internal pressure reach -0.05MPa, and the external argon pressure is adjusted to 0.05MPa, so that there is a pressure difference of 0.1MPa inside and outside the quartz tube.

[0063] The rotation speed of the copper roller was adjusted to 15m / s, and the heating current of the induction coil was adjusted. When the current reached above 35A, the alloy ingot was observed to turn red. The current was further increased to above 40A, and the alloy ingot flowed in liquid state. The molten alloy was sprayed onto the rotating copper roller by using the air pressure difference to quickly solidify and form a quick-quenching strip.

[0064] In the rapid quenching Ni 37 Co 13 Mn 35 Ti14 A temperature-induced metamagnetic martensitic phase transformation was observed in the Hf1 strip sample.

[0065] The isofield thermomagnetic curves of the samples are shown in the attached figure. Figure 1 The isothermal magnetization curves under 0-5T external magnetic field are shown in the attached Figure 2 As shown. During the measurement, the temperature was first cooled to 100K in zero field, and then magnetic fields of 0.1T and 5T were applied to measure the equifield thermomagnetic curves in the temperature range of 100K-400K. It can be seen that the alloy undergoes a drastic martensitic phase transformation between 290K-320K. During the heating process, the alloy is in a weak magnetic state at low temperature. As the temperature rises to around 316K, a reverse martensitic phase transformation from weak magnetic martensite to strong magnetic austenite occurs, and the magnetization intensity of the alloy is significantly improved.

[0066] Figure 2 In the measurement of isothermal magnetization curve, the "cycle method" is used, that is, before each temperature measurement, the temperature must be lowered by zero field to make the sample enter a weak magnetic state, and then the zero field is raised to the measurement temperature to measure the magnetization curve. Figure 2 It can be seen that a drastic magnetic field-driven martensitic phase transformation is obtained in this composition. At lower temperatures, the alloy magnetization increases slowly with the increase of the magnetic field, indicating that the alloy is in a weak magnetic state at low temperatures; while at higher temperatures, the alloy magnetization increases rapidly with the increase of the magnetic field and gradually tends to saturation, indicating that the alloy is in a ferromagnetic state at higher temperatures. In addition, according to the isothermal magnetization curves in the temperature range of 275K-316K, the calculated magnetic entropy change is shown in the attached figure. Figure 3 As shown in the figure, the strip has a maximum magnetic entropy change of 21.39 J kg under an external magnetic field of 0-5 T. -1 K -1 , which shows that Ni 37 Co 13 Mn 35 Ti 14 The Hf1 strip significantly increases the phase transition temperature while maintaining an excellent magnetocaloric effect (i.e., obtaining a large magnetic entropy change).

[0067] Example 2

[0068] Example 2 is an alloy satisfying the fourth chemical formula Ni 37 Co 13 Mn 35 Ti 15-x Ta x , the Ta doping amount is 1at.%, that is, the alloy with magnetic field driven variable magnetic martensitic phase transformation is Ni 37 Co 13 Mn 35 Ti 14 Ta1.

[0069] The preparation method of the all-d Heusler alloy with martensitic transformation temperature by adding Ta into Ni-Co-Mn-Ti in this embodiment 2 is the same as the preparation process of embodiment 1, which will not be described in detail here.

[0070] In the rapid quenching Ni 37 Co 13 Mn 35 Ti 14 Temperature-induced metamagnetic martensitic transformation was observed in Ta1 strip samples.

[0071] Under the conditions of external magnetic field of 0.1T and 5T respectively, the isofield thermomagnetic curves of magnetization intensity varying with temperature in the temperature range from 100K to 400K were measured. Figure 4 As shown in Figure 2, the strip sample undergoes a transformation from weakly magnetic martensite to ferromagnetic austenite during the heating process, and obvious thermal hysteresis can be observed. 37 Co 13 Mn 35 Ti 14 The phase transition temperature of Ta1 is 312K, which is 16K higher than the 296K of Ni-Co-Mn-Ti. Therefore, the addition of 1at.% Ta has adjusted the phase transition temperature to above room temperature, significantly widening the refrigeration temperature range. The isothermal magnetization curves under 0-5T external magnetic field are shown in the attached figure. Figure 5 In addition, according to the isothermal magnetization curves in the temperature range of 260K-314K, the calculated magnetic entropy change is shown in the attached figure. Figure 6 As shown, the strip has a maximum magnetic entropy change of 17.46 Jkg under an external magnetic field of 0-5 T. -1 K -1 , which shows that Ni 37 Co 13 Mn 35 Ti 14 The Ta1 strip significantly increases the phase transition temperature while maintaining an excellent magnetocaloric effect (i.e., obtaining a larger magnetic entropy change).

[0072] Example 3

[0073] Example 3 satisfies the fourth chemical formula of the alloy Ni 37 Co 13 Mn 35 Ti 15-x Ta x , the Ta doping amount is 2at.%, that is, the alloy Ni with magnetic field driven variable magnetic martensitic phase transformation 37 Co 13 Mn 35 Ti 13 Ta2.

[0074] The preparation method of the all-d Heusler alloy with martensitic transformation temperature by adding Ta into Ni-Co-Mn-Ti in this embodiment 3 is the same as the preparation process of embodiment 2, which will not be described in detail here.

[0075] In the rapid quenching Ni 37 Co 13 Mn 35 Ti 13 Temperature-induced metamagnetic martensitic transformation was observed in Ta2 strip samples.

[0076] Under the conditions of external magnetic field of 0.1T and 5T respectively, the isofield thermomagnetic curves of magnetization intensity varying with temperature in the temperature range from 100K to 400K were measured. Figure 7 As shown in Figure 2, the strip sample undergoes a transformation from weakly magnetic martensite to ferromagnetic austenite during the heating process, and obvious thermal hysteresis can be observed. 37 Co 13 Mn 35 Ti 13 The phase transition temperature of Ta2 is 362 K, which is 66 K higher than that of Ni-Co-Mn-Ti at 296 K. Therefore, the incorporation of 2 at.% Ta has significantly adjusted the phase transition temperature to above room temperature, significantly broadening the refrigeration temperature range.

[0077] Example 4

[0078] Example 4 is a fourth general chemical formula of the alloy Ni 37 Co 13 Mn 35 Ti 15-x Ta x , the Ta doping amount is 3at.%, that is, the alloy Ni with magnetic field driven variable magnetic martensitic phase transformation 37 Co 13 Mn 35 Ti 12 Ta3.

[0079] The preparation method of the all-d Heusler alloy with martensitic transformation temperature by adding Ta into Ni-Co-Mn-Ti in this embodiment 4 is the same as the preparation process of embodiment 2, which will not be described in detail here.

[0080] In the rapid quenching Ni 37 Co 13 Mn 35 Ti 12 Temperature-induced metamagnetic martensitic transformation was observed in Ta3 ribbon samples.

[0081] Under the conditions of external magnetic field of 0.1T and 5T respectively, the isofield thermomagnetic curves of magnetization intensity varying with temperature in the temperature range from 100K to 400K were measured. Figure 8 As shown in Figure 2, the strip sample undergoes a transformation from weakly magnetic martensite to ferromagnetic austenite during the heating process, and obvious thermal hysteresis can be observed. 37 Co 13 Mn 35 Ti 12 The phase transition temperature of Ta3 is 378 K, which is 82 K higher than the 296 K of Ni-Co-Mn-Ti. Therefore, the incorporation of 3 at.% Ta has significantly adjusted the phase transition temperature to above room temperature, significantly broadening the refrigeration temperature range.

[0082] Example 5

[0083] Example 5 is the fifth chemical formula of the alloy Ni 37 Co 13 Mn 35 Ti 15-x Mo x , Mo doping amount is 1at.%, that is, the alloy Ni with magnetic field driven variable magnetic martensitic phase transformation 37 Co 13 Mn 35 Ti 14 Mo1.

[0084] The preparation method of the all-d Heusler alloy with martensitic phase transition temperature by adding Mo into Ni-Co-Mn-Ti in this embodiment 5 is the same as the preparation process of embodiment 1, except that the equifield thermomagnetic curves are measured in the temperature range of 100K-400K by applying magnetic fields of 0.1T and 5T respectively. Fig. 9 It can be seen that the alloy undergoes a drastic martensitic phase transformation between 350K and 370K. During the heating process, the alloy is in a weak magnetic state at low temperature. As the temperature rises to around 366K, a reverse martensitic phase transformation from weak magnetic martensite to strong magnetic austenite occurs, which greatly broadens the phase transition temperature. In addition, according to the isothermal magnetization curves in the temperature range of 300K-366K (see attached Fig.10 The calculated magnetic entropy change is shown in the attached figure. Fig.11 As shown, the strip has a maximum magnetic entropy change of 12.36 J kg under an external magnetic field of 0-5 T. -1 K -1 , which shows that Ni 37 Co 13 Mn 35 Ti 14 The Mo1 strips significantly increase the phase transition temperature while maintaining excellent magnetocaloric effect (i.e., obtaining a large magnetic entropy change).

[0085] Example 6

[0086] Example 6 is the fifth chemical formula of the alloy Ni 37 Co 13 Mn 35 Ti 15-x Mo x , Mo doping amount is 2at.%, that is, the alloy Ni with magnetic field driven variable magnetic martensitic phase transformation 37 Co 13 Mn 35 Ti 13 Mo2.

[0087] The method of adding Mo to Ni-Co-Mn-Ti to significantly increase the phase transition temperature in this embodiment 6 is the same as the preparation process of embodiment 5, the only difference is that the equifield thermomagnetic curves are measured in the temperature range of 350K-600K by applying magnetic fields of 0.1T and 5T respectively. Fig.12 Under an external magnetic field of 5 T, the phase transition temperature is 410K.

[0088] Example 7

[0089] Example 7 is the fifth chemical formula of the alloy Ni 37 Co 13 Mn 35 Ti 15-x Mo x , Mo doping amount is 3at.%, that is, the alloy Ni with magnetic field driven variable magnetic martensitic phase transformation 37 Co 13 Mn 35 Ti 12 Mo3.

[0090] The preparation method of the all-d Heusler alloy with martensitic phase transition temperature doped with Mo in Ni-Co-Mn-Ti in this embodiment 7 is the same as the preparation process of embodiment 5, except that the equifield thermomagnetic curve is measured in the temperature range of 350K-700K by applying a magnetic field of 5T. Fig.13 It can be seen that the alloy undergoes a drastic martensitic phase transformation between 450K and 490K. During the heating process, the alloy is in a weak magnetic state at low temperatures, and the phase transformation temperature rises to 478K under a 5T external magnetic field. Compared with Ni 37 Co 13 Mn 35 Ti 15 , which greatly broadens the phase transition temperature, and it can be observed that the phase transition temperature shows an upward trend with the increase of Mo content.

[0091] Example 8

[0092] Example 8 is the fifth chemical formula of the alloy Ni 37 Co 13 Mn 35 Ti 15-x Mo x , Mo doping amount is 5at.%, that is, the alloy Ni with magnetic field driven variable magnetic martensitic phase transformation 37 Co 13 Mn 35 Ti 10 Mo5.

[0093] The preparation method of the all-d Heusler alloy with martensitic phase transition temperature of Ni-Co-Mn-Ti doped with Mo in this embodiment 8 is the same as the preparation process of embodiment 5, except that the equifield thermomagnetic curve is measured in the temperature range of 350K-750K by applying a magnetic field of 5T. Fig.14 It can be seen that the alloy undergoes a drastic martensitic phase transformation between 480K and 570K. During the heating process, the alloy is in a weak magnetic state at low temperatures, and the phase transformation temperature rises to 510K under a 5T external magnetic field. Compared with Ni 37 Co 13 Mn 35 Ti 15 , greatly broadening the phase transition temperature.

[0094] Example 9

[0095] Example 9 is the fifth chemical formula of the alloy Ni 37 Co 13 Mn 35 Ti 15-x Mo x , Mo doping amount is 7at.%, that is, the alloy Ni with magnetic field driven variable magnetic martensitic phase transformation 37 Co 13 Mn 35 Ti8Mo7.

[0096] The preparation method of the all-d Heusler alloy with martensitic phase transition temperature of Ni-Co-Mn-Ti doped with Mo in this embodiment 9 is the same as the preparation process of embodiment 5, except that the equifield thermomagnetic curve is measured in the temperature range of 350K-850K by applying a magnetic field of 5T. Fig.15 It can be seen that the alloy undergoes a drastic martensitic phase transformation between 400K and 510K. During the heating process, the alloy is in a weak magnetic state at low temperatures, and the phase transformation temperature rises to 484K under a 5T external magnetic field.

[0097] Example 10

[0098] Example 10 is the fifth chemical formula of the alloy Ni 37 Co13 Mn 35 Ti 15-x Mo x , Mo doping amount is 9at.%, that is, the alloy Ni with magnetic field driven variable magnetic martensitic phase transformation 37 Co 13 Mn 35 Ti6Mo9.

[0099] The preparation method of the all-d Heusler alloy with martensitic phase transition temperature of Ni-Co-Mn-Ti doped with Mo in this embodiment 10 is the same as the preparation process of embodiment 5, except that the equifield thermomagnetic curve is measured in the temperature range of 350K-850K by applying a magnetic field of 5T. Fig.16 The phase transition temperature under an external magnetic field of 5 T rises to 574K, which is far above room temperature and greatly broadens the refrigeration temperature range.

[0100] According to Ni 37 Co 13 Mn 35 Ti 14 The stoichiometric ratio of T1 (T = Zr, Nb, Hf, Ta, Mo, W) is used to calculate the required mass of Ni, Co, Mn, Ti, Zr, Nb, Hf, Ta, Mo, and W elements for batching; the belt speed is 15 m / s. 37 Co 13 Mn 35 Ti 14 A magnetic field-driven drastic magnetic martensitic phase transformation is obtained in the T1 alloy sample, and a large magnetic entropy change is obtained near the phase transition temperature.

[0101] Embodiment 11

[0102] Example 11 is the fifth chemical formula of the alloy Ni 37 Co 13 Mn 35 Ti 15-x Mo x , Mo doping amount is 0at.%, that is, the alloy Ni with magnetic field driven variable magnetic martensitic phase transformation 37 Co 13 Mn 35 Ti 15 The equifield thermomagnetic curves of the samples are shown in the attached Fig.17 shown.

[0103] From the attached Figure 1 -Attached Fig.17It can be found that any one of the Ni-Co-Mn-Ti based Heusler alloys that realizes the variable magnetic reverse martensitic phase transformation in Examples 1 to 11 has the above-mentioned property of causing the material to undergo a martensitic phase transformation between a weakly magnetic martensite phase and a strongly magnetic austenite phase under the conditions of temperature, magnetic field or pressure (internal pressure or external pressure). It can be inferred that the above three general formula Ni-Co-Mn-Ti based Heusler alloys can realize a magnetic field-driven variable magnetic reverse martensitic phase transformation while undergoing a temperature-driven martensitic phase transformation.

[0104] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. An all-d Heusler alloy capable of significantly increasing the martensitic transformation temperature, characterized in that: The chemical formula of the all-d Heusler alloy capable of significantly increasing the martensitic transformation temperature is Ni 37 Co 13 Mn 35 Ti 15-x T x , wherein 0≤x≤15, x represents the atomic percentage content, T is a 4d or 5d transition group high melting point metal, and the 4d or 5d transition group high melting point metal is any one of Zr, Nb, Hf, Ta, Mo, and W.

2. An all-d Heusler alloy capable of significantly increasing the martensitic transformation temperature as claimed in claim 1, characterized in that: When the introduced transition metal with high melting point is Zr, the chemical formula of the alloy is Ni 37 Co 13 Mn 35 Ti 15-x Zr x , where 0≤x≤15; or When the introduced transition metal with high melting point is Nb, the chemical formula of the alloy is Ni 37 Co 13 Mn 35 Ti 15-x Nb x , where 0≤x≤15; or When the introduced transition metal with high melting point is Hf, the chemical formula of the alloy is Ni 37 Co 13 Mn 35 Ti 15-x Hf x , where 0≤x≤15; or When the introduced transition metal with high melting point is Ta, the chemical formula of the alloy is Ni 37 Co 13 Mn 35 Ti 15-x Ta x , where 0≤x≤15; or When the introduced transition metal with high melting point is Mo, the chemical formula of the alloy is Ni 37 Co 13 Mn 35 Ti 15-x Mo x , where 0≤x≤15 or When the introduced transition metal with high melting point is W, the chemical formula of the alloy is Ni 37 Co 13 Mn 35 Ti 15-x W x , where 0≤x≤15.

3. The method for preparing an all-d Heusler alloy capable of significantly increasing the martensitic transformation temperature as claimed in claim 1, characterized in that: The method is to introduce any 4d, 5d transition group high melting point metal of Zr, Nb, Hf, Ta, Mo, W into the Ni-Co-Mn-Ti Heusler alloy, so that the alloy is doped with the 4d, 5d transition group high melting point metal so that the introduced metal forms a new covalent bond to adjust the magnetization intensity of the alloy and the sensitivity of the martensitic phase transformation to the magnetic field, and realize the magnetic field-driven variable magnetism reverse martensitic phase transformation while the temperature-driven martensitic phase transformation occurs.

4. A method for preparing an all-d Heusler alloy capable of significantly increasing the martensitic transformation temperature as claimed in claim 3, characterized in that: The steps include: Calculate the mass of any one 4d or 5d transition group high melting point metal element of Ni, Co, Mn, Ti, Zr, Nb, Hf, Ta, Mo, or W required according to the stoichiometric ratio, and prepare the ingredients; Arc melting was used to obtain alloy ingot samples; The surface of some alloy ingot samples obtained above was polished, placed in a quartz tube with an opening diameter of 1 mm at one end, and placed in a high vacuum belt spinning device. The vacuum degree was drawn to 8×10 -4 Pa, argon is filled into the belt-spinning furnace to make the internal pressure reach -0.05MPa, and the external argon pressure is adjusted to 0.05MPa, so that there is a pressure difference of 0.1MPa inside and outside the quartz tube; The rotation speed of the copper roller and the heating current of the induction coil are adjusted, and the molten alloy is sprayed onto the rotating copper roller by using the air pressure difference to quickly solidify and form a fast-quenching strip with uniform composition and structure.

5. A method for preparing an all-dHeusler alloy capable of significantly increasing the martensitic transformation temperature as claimed in claim 4, characterized in that: The doping amount of any one 4d, 5d transition group high melting point metal single substance of Zr, Nb, Hf, Ta, Mo, and W is 1at.%-15at.%.

6. A method for preparing an all-d Heusler alloy capable of significantly increasing the martensitic transformation temperature as claimed in claim 4, characterized in that: The mass of any 4d, 5d transition group high melting point metal single substance among Ni, Co, Mn, Ti, Zr, Nb, Hf, Ta, Mo, and W needs to be accurate to two decimal places in milligrams, and the purity of the single substance needs to be controlled at more than 99.99%.

7. A method for preparing an all-d Heusler alloy capable of significantly increasing the martensitic transformation temperature as claimed in claim 4, characterized in that: During the arc melting, the raw materials are placed in a water-cooled copper crucible arc furnace, 0.03 Pa of argon gas is filled into the furnace for washing, and then the vacuum degree is drawn to 5×10 -3 Pa, fill with 0.7 atmospheres of argon gas with a purity of 99.999% for arc melting; For the first smelting, use 50A-70A current to melt the metal. When the metal in the crucible flows in liquid state, the first smelting is completed and turned over. Increase the current to 100A-105A and smelt 4 more times to obtain the alloy ingot.

8. A method for preparing an all-d Heusler alloy capable of significantly increasing the martensitic transformation temperature as claimed in claim 4, characterized in that: The molten alloy is sprayed onto the rotating copper roller by using air pressure difference to quickly solidify and form a quick-quenching strip. The copper roller speed and induction coil heating current conditions are as follows: the copper roller speed is 15m / s, and when the induction coil heating current reaches 35A or more, the alloy ingot turns red. Continue to increase the current to more than 40A until the alloy ingot flows in liquid state.

9. An application of the all-dHeusler alloy of claim 1 that can significantly increase the martensitic phase transition temperature in the preparation of magnetic storage devices, magnetic drives, temperature sensitive elements, magnetic sensitive elements, magnetic heat pumps, magnetic sensors, thermomagnetic electric conversion devices, and solid-state refrigeration devices.

Citation Information

Patent Citations

  • Preparation method for magnetic phase-change alloy

    CN105695802A

  • Material capable of regulating and controlling magnetism and related magnetic effects through bending or twisting, preparation method of material and application of material

    CN111210959A

  • Magnetocaloric effect enhancing material and preparation method thereof

    CN112216458A

  • Fe-BASED FERROMAGNETIC SHAPE MEMORY ALLOY AND APPLICATION THEREOF

    JP2011042852A

  • Highly tunable, inexpensive and easily fabricated magnetocaloric materials

    US20190214169A1

Cited By

  • Smelting method of Heusler alloy Co2MnAl

    CN120989386A