X80 steel plate for conveying coal gas and manufacturing method thereof
By designing specific chemical components and process flows, a structure dominated by acupuncture ferrite is formed, which solves the corrosive damage problem of coal-to-gas hydrogen to steel plates in the prior art, and achieves the excellent performance of steel plates in high hydrogen environments.
Patent Information
- Application Number
- CN202410917608.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
There is a lack of X80 steel plate suitable for transporting coal-to-gas in the prior art. The hydrogen in coal-to-gas causes corrosive damage to metal materials, affecting the service environment and conditions of the pipeline.
A X80 steel plate with chemical compositions C: 0.02-0.05%, Mn: 1.35-1.75%, etc. was designed, and a specific process flow includes converter smelting, LF refining, RH vacuum refining, continuous casting, reheating, and specific TMCP process. and cooling process, a structure dominated by acupuncture ferrite is formed to enhance anti-hydrogen embrittlement and toughness.
The steel plate has excellent yield and tensile strength under simulated 1MPa hydrogen partial pressure, and has good anti-damage properties caused by hydrogen, and is suitable for coal-to-gas service environment.
Smart Images

Figure CN118932253A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of special steel smelting, and specifically relates to an X80 steel plate for conveying coal-to-gas and a manufacturing method thereof. Background Art
[0002] Energy security is related to national security. The country has initiated energy security and green energy construction. Among my country's fossil energy, oil is relatively scarce and mainly relies on imports, but my country's coal resources are relatively abundant. In order to supplement natural gas, coal-to-gas is a good development direction. However, compared with ordinary natural gas, coal-to-gas contains a certain amount of H, which is a common corrosive element and causes hydrogen damage to metal materials, which will affect the service environment and conditions of pipelines.
[0003] At present, there are few public reports on patents related to X80 pipeline steel plates for coal-to-gas. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide an X80 steel plate for conveying coal-to-gas and a manufacturing method thereof in view of the above-mentioned prior art.
[0005] The technical solution adopted by the present invention to solve the above problem is: an X80 steel plate for conveying coal gas, the chemical composition of the steel plate is C: 0.02-0.05%, Mn: 1.35-1.75%, Si: ≤0.35%, S: ≤0.001%, P: ≤0.012%, Nb: 0.04-0.07%, Ti: ≤0.012%, V: 0.03-0.06%, Alt: 0.05-0.08%, N: ≤0.0030%, O: ≤0.003%, Pb ≤0.0015%, Zn ≤0.003%, Sb ≤0.0015%, Sn ≤0.0015%, Cr: 0.10-0.25%, Ni: ≤1.0%; Mo: 0.08-0.13% Ca: ≤0.015%, Cu: ≤0.12-0.25%, Ca / S: 1.1-2.0, the balance is Fe and unavoidable impurity elements; the thickness of the steel plate is not higher than 35 mm.
[0006] The steel plate has a yield strength of ≥530 MPa, a tensile strength of ≥675 MPa, a yield strength ratio of ≤0.84, an impact energy of -30°C of ≥420 J, an impact energy of -60°C of ≥400 J, a drop hammer shear area of -20°C of ≥85%, a drop hammer shear area of -25°C of ≥85%, an aging impact energy of -30°C of ≥350 J, a yield strength of no higher than 645 MPa, a tensile strength of no higher than 720 MPa, a good hydrogen charging slow tensile test after pre-deformation, and excellent HIC resistance.
[0007] The composition design principle of the present invention is to fully consider the influence of H on the performance of the steel plate after H filling, adopt appropriate composition design, and combine with specific processes to obtain a structure suitable for coal gasification service environment. Its structure is characterized by mainly acicular ferrite and a small amount of polygonal or quasi-polygonal ferrite structure, thereby obtaining excellent performance. The main basic elements have the following functions:
[0008] C: C is the most economical and basic strengthening element in steel. It can significantly improve the strength of steel through solid solution strengthening and precipitation strengthening, but it has an adverse effect on the toughness, ductility and welding performance of steel. Therefore, the development trend of pipeline steel is to continuously reduce the C content. Considering the matching relationship between strength and toughness, the C content is controlled at 0.02-0.05%.
[0009] Mn: It improves the strength of steel through solid solution strengthening. It is the most important element in pipeline steel to make up for the strength loss caused by the reduction of C content. Mn is also an element that expands the γ phase region, which can reduce the γ→α phase transition temperature of steel, help to obtain fine phase transformation products, improve the toughness of steel, and reduce the toughness-brittleness transition temperature. Mn is also an element that improves the hardenability of steel. Considering that it was found during the inspection process that Mn segregation has an adverse effect on the drop hammer performance, while taking into account the strength requirements, the Mn content in the present invention is designed to be in the range of (1.35-1.75%, in order to alleviate the central segregation caused by the high Mn content, light pressure is used during continuous casting.
[0010] Nb: It is one of the most important microalloying elements in modern microalloyed steel, especially pipeline steel, and has a significant effect on grain refinement. Through Nb solid solution drag and Nb (C, N) strain induced precipitation during hot rolling, it can hinder the recovery and recrystallization of deformed austenite. Through TMCP, the deformed austenite rolled in the non-recrystallized zone is transformed into fine phase transformation products during phase transformation, so that the steel has high strength and high toughness.
[0011] V: Usually, the precipitation of V and the weak grain refinement effect are used, but the present patent mainly uses the precipitates of V to form effective hydrogen traps, which is beneficial to weaken the tendency of hydrogen embrittlement. However, too high V will be detrimental to toughness. The present patent sets V at 0.03-0.06%.
[0012] Ti: It is a strong N-fixing element with a Ti / N stoichiometric ratio of 3.42. About 0.01% Ti can fix less than 20ppm of N in steel, and a TiN precipitation phase can be formed during the slab continuous casting process. This fine precipitation phase can effectively prevent the growth of austenite grains during the heating process of the slab, help to increase the solid solubility of Nb in austenite, and improve the impact toughness of the heat affected zone of welding. It is an indispensable element in pipeline steel, but too high Ti will form large TiN particles, affecting the drop hammer performance. Therefore, this patent application sets Ti≤0.012%.
[0013] Al:Al is usually used as a grain refining element. This patent mainly considers the combination of Al and N to further fix the free N in the steel.
[0014] S, P: are inevitable impurity elements in pipeline steel. It is hoped that the lower the better. By changing the sulfide form through ultra-low sulfur and Ca treatment, the pipeline steel can have high impact toughness.
[0015] Cr: The addition of Cr can improve the hardenability of steel and is relatively economical.
[0016] Cu: Cu is used to form a Cu-rich phase, which is conducive to the formation of hydrogen traps, thereby avoiding local hydrogen embrittlement, but the Cu content cannot be too high. The Cu content of this patent application is 0.12-0.25%
[0017] Mo: Mo is added mainly to obtain acicular ferrite, but too high Mo is sensitive to the formation of lower bainite or martensite, so Mo is controlled at 0.08-0.13%.
[0018] The present invention also relates to a method for manufacturing X80 steel grade pipeline steel plate for coal gas transportation, the process flow of which includes: proportioning and preparing materials → smelting in a converter or electric furnace → refining outside the furnace → continuous casting → slab reheating → specific TMCP process + stack cooling after cooling → straightening. The specific steps of the manufacturing method are as follows:
[0019] First, the smelting raw materials are sequentially subjected to KR molten iron pretreatment, converter smelting, LF refining, RH vacuum refining and continuous casting to produce continuous casting billets that meet the chemical composition requirements and have a thickness of no less than 350 mm;
[0020] Soft reduction is used during continuous casting to improve the core segregation caused by high Mn.
[0021] The continuous casting billet is reheated to no higher than 1180°C and subjected to a specific TMCP process + water cooling + pile cooling + straightening.
[0022] The specific TMCP process includes two-stage rolling and intermediate billet cooling: the first stage is recrystallization zone rolling, the final rolling temperature is controlled to be no higher than 1150°C, and the single pass reduction rate of two to three consecutive passes is controlled to be no less than 20% during recrystallization zone rolling;
[0023] The second stage is rolling in the non-recrystallization zone, and the starting rolling temperature is not higher than 880℃.
[0024] The final rolling temperature is controlled at Ar3±20℃
[0025] After rolling, the steel plate is cooled by water cooling, the initial cooling temperature is controlled at Ar3-20~Ar3-40℃, the final cooling temperature is not higher than 400℃, and the cooling rate is 10~35℃ / s; after cooling, it is straightened and finally directly cooled to room temperature to obtain the finished steel plate.
[0026] Compared with the prior art, the advantages of the present invention are:
[0027] According to the mechanism of H traps and H damage, the present invention controls the use of the second phase formed by certain elements in the body to form effective traps to promote the uniform distribution of hydrogen, thereby avoiding the occurrence of local hydrogen embrittlement. On the other hand, it is necessary to obtain a structure that is mainly acicular ferrite and contains a small amount of quasi-polygonal ferrite, which is beneficial to improving the plasticity under a certain H concentration. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram of the metallographic structure of the present invention. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is described in more detail in conjunction with the preferred embodiments of the present invention. However, these embodiments are only descriptions of the preferred implementation methods of the present invention and cannot impose any limitation on the scope of the present invention.
[0030] The embodiment of the present invention relates to an X80 steel grade pipeline steel plate for conveying coal gas and a manufacturing method thereof as follows:
[0031] Proportioning and preparing materials → smelting in converter or electric furnace → refining outside the furnace → continuous casting → slab reheating → specific TMCP process + stack cooling after cooling → straightening.
[0032] The specific process steps are as follows: the smelting raw materials are sequentially subjected to KR hot metal pretreatment, converter smelting, LF refining, RH vacuum refining and continuous casting. The light reduction process is used during continuous casting to improve the core segregation caused by the high Mn content. A continuous casting billet with a thickness of 350mm that meets the chemical composition requirements is manufactured; the continuous casting billet is reheated to no more than 1180℃ and subjected to a specific TMCP process + water cooling + stack cooling + straightening.
[0033] The specific TMCP process includes two-stage rolling: the first stage is recrystallization zone rolling, the final rolling temperature is controlled to be no higher than 1150°C, and the single pass reduction rate of two to three consecutive passes is controlled to be no less than 20% during recrystallization zone rolling;
[0034] The second stage is rolling in the non-recrystallization zone, the starting rolling temperature is not higher than 880°C, and the final rolling temperature is controlled at the phase transformation critical temperature Ar3-10°C.
[0035] After rolling, the steel plate is cooled by water cooling, the starting cooling temperature is controlled to be no higher than Ar3-25°C, the ending cooling temperature is controlled to be no higher than 400°C, and the cooling rate is 19°C / s; after the water cooling is completed, it is straightened and finally directly cooled to room temperature to obtain the finished steel plate.
[0036] The specific chemical composition of the steel plates involved in each embodiment is shown in Table 1, the specific TMCP process parameters are shown in Table 2, the main mechanical properties are shown in Table 3, and the main mechanical properties of the equivalent hydrogen-filled slow tensile test under a hydrogen partial pressure of 1 MPa are shown in Table 4.
[0037] Table 1
[0038]
[0039] Table 2
[0040]
[0041]
[0042] Table 3
[0043]
[0044] Table 4
[0045]
[0046] Although the preferred embodiments of the present invention are described in detail above, it should be clearly understood that various modifications and variations are possible for those skilled in the art. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An X80 steel plate for coal gasification, characterized in that: The chemical composition of the steel plate is calculated by mass percentage as follows: C: 0.02-0.05%, Mn: 1.35-1.75%, Si: ≤0.35%, S: ≤0.001%, P: ≤0.012%, Nb: 0.04-0.07%, Ti: ≤0.012%, V: 0.03-0.06%, Alt: 0.05-0.08%, N: ≤0.0030%, O: ≤ 0.003%, Pb≤0.0015%, Zn≤0.003%, Sb≤0.0015%, Sn≤0.0015%, Cr: 0.10-0.25%, Ni: ≤1.0%; Mo; 0.08-0.13% Ca: ≤0.015%, Cu: ≤0.15-0.25%, Ca / S: 1.1-2.0, the balance is Fe and unavoidable impurity elements.
2. The X80 steel plate for coal gasification according to claim 1, characterized in that: The thickness of the steel plate is not more than 35 mm.
3. The X80 steel plate for coal gasification according to claim 1, characterized in that: The metallographic structure of the steel plate is mainly composed of acicular ferrite, and a small amount of polygonal or quasi-polygonal ferrite is distributed.
4. The X80 steel plate for coal gasification according to claim 1, characterized in that: The steel plate has a yield strength of ≥530Mpa; a tensile strength of ≥675Mpa, a yield strength ratio of ≤0.84, an impact energy at -30°C of ≥420J, an impact energy at -60°C of ≥400J, a drop weight shear area at -20°C of ≥85%, a drop weight shear area at -25°C of ≥85%. The aging impact energy at -30°C is ≥350J, and the yield strength under an electrochemical hydrogen charging slow pull test simulating a hydrogen partial pressure of not less than 1MPa is not higher than 645MPa, and the tensile strength is not higher than 720MPa.
5. A method for manufacturing an X80 steel plate for coal gasification according to claim 1, characterized in that: The method specifically comprises the following steps: Step 1: First, the smelting raw materials are sequentially subjected to KR molten iron pretreatment, converter smelting, LF refining, RH vacuum refining and continuous casting to produce a continuous casting billet that meets the chemical composition requirements and has a thickness of not less than 350 mm; Step 2: reheat the continuous casting billet to no higher than 1180°C, and perform TMCP process + water cooling + pile cooling + straightening; Step 3: The TMCP process includes two-stage rolling and intermediate billet cooling: the first stage is rolling in the recrystallization zone, and the final rolling temperature is controlled at no more than 1150°C; the second stage is rolling in the non-recrystallization zone, and the start rolling temperature is no more than 880°C; the final rolling temperature is controlled at Ar3±20°C. Step 4: Cool the steel plate by water cooling after rolling, control the starting cooling temperature to be Ar3-20~Ar3-40℃, end cooling temperature to be no higher than 400℃, and cooling rate to be 10~35℃ / s; straighten after cooling, and finally cool directly to room temperature to obtain the finished steel plate.
6. The method for manufacturing X80 steel plate for coal gasification according to claim 5, characterized in that: During recrystallization zone rolling, the reduction rate of a single pass is controlled to be no less than 20% for two to three consecutive passes.