Non-isothermal treatment method for improving annealing softening resistance and yield ratio of aluminum alloy

The dissolution and uniform distribution of the second phase in the Al-Mg-based aluminum alloy by non-isothermal treatment method was solved, and the mechanical properties and strength of the aluminum alloy were significantly improved.

CN118932261APending Publication Date: 2024-11-12KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411031862.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Al-Mg-based aluminum alloys are prone to problems such as annealing softening and low yield strength ratio during heat treatment, resulting in a decrease in alloy strength. It is difficult for existing isothermal annealing methods to effectively solve these problems.

Method used

The non-isothermal treatment method is adopted to significantly improve the mechanical properties of the aluminum alloy by dissolving and uniform distribution of the second phase within different temperature intervals. The specific steps include heating to a preset temperature at a constant speed and heating and cooling treatment at different temperature segments to ensure uniform distribution and stable tissue of the second phase.

Benefits of technology

In a short time, the tensile strength and yield strength ratio of aluminum alloy are significantly improved, the mechanical properties and service performance of aluminum alloy are significantly improved, and the impact of annealing and softening is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932261A_ABST
    Figure CN118932261A_ABST
Patent Text Reader

Abstract

The invention relates to a non-isothermal treatment method for improving annealing softening resistance and yield ratio of an aluminum alloy, and belongs to the technical field of aluminum alloy heat treatment. The method comprises the following steps: uniformly heating the aluminum alloy to a preset temperature T1 at a heating rate of 8-9 DEG C / min; then heating to a preset temperature T2 at a constant speed at a heating rate of 1.7-3.3 DEG C / min; uniformly heating to a final preset temperature T3 at a heating rate of 0.6-1.4 DEG C / min; and finally, cooling to room temperature at a constant speed of 0.5-5 DEG C / min. According to the method, the annealing softening resisting behavior of the aluminum alloy can be effectively improved within a short time by enhancing dispersion and precipitation of a second phase in the aluminum alloy and improving the annealing softening resisting behavior, meanwhile, the strength of the alloy is improved, the higher yield ratio of the alloy is obtained, and the mechanical property of the aluminum alloy can be remarkably improved by adopting a reasonable non-isothermal process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a non-isothermal treatment method for improving the annealing softening resistance of aluminum alloy and increasing the yield ratio, belonging to the technical field of aluminum alloy heat treatment. Background Art

[0002] Aluminum alloys have become one of the key materials for lightweight structures due to their high specific strength, excellent corrosion resistance and good machinability. They are widely used in aerospace, automobile lightweight and high-speed rail transportation. Generally, the addition of alloying elements, deformation strengthening and corresponding heat treatment technologies are the basic means to improve the performance of aluminum alloys. However, in Al-Mg aluminum alloys, due to the unsatisfactory effects of solid solution strengthening and dispersion strengthening, it is difficult for conventional heat treatment to achieve the expected results. Therefore, Al-Mg aluminum alloys usually improve their mechanical properties through deformation processes. However, during the deformation process, a large number of dislocation entanglements are generated in the alloy, and dislocation bundles and dislocation networks are gradually formed, resulting in defects such as structural instability and stress concentration in the alloy. Generally, subsequent annealing is required to improve the deformed structure. However, annealing will weaken the contribution of rolling to the strength of the alloy, and reduce the plasticity of the material due to the suppression of dislocation strengthening, which will cause the alloy to soften during annealing, thereby reducing the strength of the alloy. Summary of the invention

[0003] In view of the problems of annealing softening and low yield strength ratio of aluminum alloy in the prior art, the present invention proposes a non-isothermal treatment method for improving the annealing softening resistance of aluminum alloy and increasing the yield strength ratio, and improving the annealing softening problem of aluminum alloy by enhancing the dispersion precipitation of the second phase in the aluminum alloy to obtain a uniformly distributed second phase structure; compared with the isothermal annealing adopted in the existing treatment method, the present invention can effectively improve the annealing softening behavior of the aluminum alloy and at the same time improve the strength of the alloy in a relatively short time, so that it can obtain a better yield strength ratio, and the use of a reasonable non-isothermal process can significantly improve the mechanical properties of the aluminum alloy.

[0004] A non-isothermal treatment method for improving the annealing softening resistance of aluminum alloy and increasing the yield ratio, the specific steps are as follows:

[0005] (1) uniformly heating the aluminum alloy to a preset temperature T1 at a heating rate of 8 to 9 °C / min;

[0006] (2) uniformly heating the aluminum alloy treated in step (1) to a preset temperature T2 at a heating rate of 1.7 to 3.3° C. / min;

[0007] (3) uniformly heating the aluminum alloy treated in step (2) at a heating rate of 0.6 to 1.4° C. / min to a final preset temperature T3;

[0008] (4) The aluminum alloy treated in step (3) is uniformly cooled to room temperature at a cooling rate of 0.5 to 5°C / min.

[0009] The preset temperature T1 of step (1) is 180-200°C.

[0010] The preset temperature T2 of step (2) is 280-300°C.

[0011] The preset temperature T3 of step (3) is 325-400°C.

[0012] The total time of step (1), step (2) and step (3) is 120 to 150 minutes.

[0013] The principle of the non-isothermal process of improving the annealing softening resistance of aluminum alloy and increasing the yield ratio of the present invention is as follows:

[0014] The second phase is dissolved in different temperature ranges, the overall heating time is controlled to make it fully dissolved in the matrix, the cooling rate is controlled to precipitate a dispersed and uniform second phase structure, and the dispersion strengthening effect of the second phase is enhanced. The heating process is accompanied by the stabilization of the structure and the elimination of residual stress, and the alloy structure is uniform, reducing the influence of annealing softening, improving the mechanical properties of the alloy, especially improving the strength and yield strength ratio of the aluminum alloy.

[0015] The beneficial effects of the present invention are:

[0016] (1) The present invention improves the annealing softening resistance of the aluminum alloy and increases the yield strength ratio by enhancing the dispersion precipitation of the second phase in the aluminum alloy.

[0017] (2) Compared with the isothermal process used in the existing treatment methods, the present invention can effectively improve the strength of the alloy in a shorter time, so that it can obtain a better yield strength ratio. The use of a reasonable non-isothermal process can significantly improve the mechanical properties and service performance of the aluminum alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a non-isothermal treatment process diagram of the present invention;

[0019] Figure 2 Isothermal treatment process diagram for comparative example;

[0020] Figure 3 This is the SEM image of the aluminum alloy microstructure of the non-isothermal treatment of Example 2;

[0021] Figure 4 This is the SEM image of the isothermally treated aluminum alloy microstructure of Comparative Example 2;

[0022] Figure 5 It is a comparison chart of tensile strength between Examples 1 to 3 and Comparative Examples 1 to 3;

[0023] Figure 6 It is a comparison chart of the yield strength ratio of Examples 1 to 3 and Comparative Examples 1 to 3. DETAILED DESCRIPTION

[0024] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.

[0025] The aluminum alloy composition in the embodiment of the present invention is within the standard composition range specified in GB T3190-2020; the SEM image of the sample is characterized by a field emission scanning electron microscope (FE-SEM, JSE-7899F), and the mechanical properties (tensile strength, yield strength ratio) of the sample are tested using a universal testing machine (SHIMADZU-AGX-100kNV).

[0026] Comparative Example 1: Aluminum alloy isothermal treatment method (see Figure 2 ), the specific steps are as follows:

[0027] The aluminum alloy was uniformly heated to 325°C at a heating rate of 20°C / min, kept at that temperature for 120 minutes, and then uniformly cooled to room temperature at a cooling rate of 0.5°C / min;

[0028] The tensile strength of the aluminum alloy after isothermal treatment is 345MPa (see Figure 5 ), the yield strength ratio is 0.63 (see Figure 6 ).

[0029] Example 1: A non-isothermal treatment method for improving the annealing softening resistance of aluminum alloy and increasing the yield strength ratio (see Figure 1 ), the specific steps are as follows:

[0030] (1) The aluminum alloy sample was uniformly heated to a preset temperature T1 (180°C) at a heating rate of 8°C / min to uniformly preheat the aluminum alloy sample and eliminate the structural defects and residual stress during the deformation process;

[0031] (2) uniformly heating the aluminum alloy sample treated in step (1) to a preset temperature T2 (280° C.) at a heating rate of 3.3° C. / min, so that a portion of the second phase in the aluminum alloy sample is dissolved;

[0032] (3) the aluminum alloy treated in step (2) is uniformly heated to a final preset temperature T3 (325°C) at a heating rate of 0.6°C / min, so as to fully complete the dissolution of the second phase in this temperature range at the preset temperature of 325°C; the total time of step (1), step (2) and step (3) is 120 minutes;

[0033] (4) cooling the aluminum alloy treated in step (3) to room temperature at a cooling rate of 0.5° C. / min; controlling the cooling rate to precipitate a uniformly dispersed second phase and retaining it at room temperature;

[0034] The tensile strength of the aluminum alloy subjected to non-isothermal treatment in this embodiment is 382 MPa (see Figure 5 ), the yield strength ratio is 0.72 (see Figure 6 ); Compared with Comparative Example 1, the tensile strength of the aluminum alloy is increased by 10.7%, and the yield strength ratio is increased by 14%.

[0035] Comparative Example 2: Aluminum alloy isothermal treatment method (see Figure 2 ), the specific steps are as follows:

[0036] The aluminum alloy was uniformly heated to 350°C at a heating rate of 20°C / min, kept at that temperature for 135 min, and then cooled to room temperature at a rate of 2.5°C / min;

[0037] The tensile strength of the aluminum alloy after isothermal treatment is 340MPa (see Figure 5 ), the yield strength ratio is 0.61 (see Figure 6 ).

[0038] Example 2: A non-isothermal treatment method for improving the annealing softening resistance of aluminum alloy and increasing the yield strength ratio (see Figure 1 ), the specific steps are as follows:

[0039] (1) The aluminum alloy sample is uniformly heated to a preset temperature T1 (190°C) at a heating rate of 8.5°C / min to uniformly preheat the aluminum alloy sample and eliminate the structural defects and residual stresses during the deformation process;

[0040] (2) uniformly heating the aluminum alloy sample treated in step (1) to a preset temperature T2 (290° C.) at a heating rate of 2.2° C. / min, so that a portion of the second phase in the aluminum alloy sample is dissolved;

[0041] (3) uniformly heating the aluminum alloy treated in step (2) to a final preset temperature T3 (350° C.) at a heating rate of 0.9° C. / min, so as to fully complete the dissolution of the second phase in this temperature range at the preset temperature of 350° C.; the total time of steps (1), (2) and (3) is 135 min;

[0042] (4) The aluminum alloy treated in step (3) is uniformly cooled to room temperature at a cooling rate of 2.5°C / min; the cooling rate is controlled to precipitate a dispersed and uniform second phase and retain it to room temperature.

[0043] The tensile strength of the aluminum alloy subjected to non-isothermal treatment in this embodiment is 379 MPa (see Figure 5 ), the yield strength ratio is 0.70 (see Figure 6 ); Compared with Comparative Example 2, the tensile strength of the aluminum alloy is increased by 11.5%, and the yield strength ratio is increased by 15%.

[0044] The SEM microstructure of the isothermally treated aluminum alloy of Comparative Example 2 is shown in Figure 3 The SEM microstructure of the aluminum alloy subjected to non-isothermal treatment in Example 2 is shown in Figure 4 ,from Figure 3 and 4 It can be seen that the amount of the second phase in the microstructure of the comparative example is small, and the size is concentrated between 1 and 1.5 μm. Compared with comparative example 2, the amount of the second phase in the microstructure of embodiment 2 is significantly increased, and the size is concentrated between 0.1 and 0.5 μm. Therefore, the dispersion strengthening effect of the second phase is enhanced, and the alloy strength is higher than that of the comparative example.

[0045] Comparative Example 3: Aluminum alloy isothermal treatment method (see Figure 2 ), the specific steps are as follows:

[0046] The aluminum alloy was heated to 400°C at a heating rate of 20°C / min, kept at this temperature for 150 min, and then cooled to room temperature at a rate of 5°C / min;

[0047] The tensile strength of the aluminum alloy after isothermal treatment is 284MPa (see Figure 5 ), the yield strength ratio is 0.50 (see Figure 6 ).

[0048] Example 3: A non-isothermal treatment method for improving the annealing softening resistance of aluminum alloy and increasing the yield strength ratio (see Figure 1 ), the specific steps are as follows:

[0049] (1) The aluminum alloy sample is uniformly heated to a preset temperature T1 (200°C) at a heating rate of 9°C / min to uniformly preheat the aluminum alloy sample and eliminate the structural defects and residual stresses during the deformation process;

[0050] (2) uniformly heating the aluminum alloy sample treated in step (1) to a preset temperature T2 (300° C.) at a heating rate of 1.7° C. / min, so that a portion of the second phase in the aluminum alloy sample is dissolved;

[0051] (3) uniformly heating the aluminum alloy treated in step (2) to a final preset temperature T3 (400° C.) at a heating rate of 1.4° C. / min, so as to fully complete the dissolution of the second phase in this temperature range at the preset temperature of 400° C.; the total time of steps (1), (2) and (3) is 150 min;

[0052] (4) cooling the aluminum alloy treated in step (3) to room temperature at a cooling rate of 5° C. / min; controlling the cooling rate to precipitate a uniformly dispersed second phase and retaining it at room temperature;

[0053] The tensile strength of the aluminum alloy subjected to non-isothermal treatment in this embodiment is 365 MPa (see Figure 5), the yield strength ratio is 0.68 (see Figure 6 ); Compared with Comparative Example 3, the tensile strength of the aluminum alloy is increased by 28.5%, and the yield strength ratio is increased by 36%.

[0054] The specific implementation modes of the present invention are described in detail above, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.

Claims

1. A non-isothermal treatment method for improving the annealing softening resistance of aluminum alloy and increasing the yield ratio, characterized in that: The specific steps are as follows: (1) uniformly heating the aluminum alloy to a preset temperature T1 at a heating rate of 8 to 9 °C / min; (2) uniformly heating the aluminum alloy treated in step (1) to a preset temperature T2 at a heating rate of 1.7 to 3.3° C. / min; (3) uniformly heating the aluminum alloy treated in step (2) at a heating rate of 0.6 to 1.4° C. / min to a final preset temperature T3; (4) The aluminum alloy treated in step (3) is uniformly cooled to room temperature at a cooling rate of 0.5 to 5°C / min.

2. The non-isothermal treatment method for improving the annealing softening resistance and yield ratio of aluminum alloy according to claim 1, characterized in that: The preset temperature T1 of step (1) is 180-200°C.

3. The non-isothermal treatment method for improving the annealing softening resistance and yield ratio of aluminum alloy according to claim 1, characterized in that: The preset temperature T2 of step (2) is 280-300°C.

4. The non-isothermal treatment method for improving the annealing softening resistance and yield ratio of aluminum alloy according to claim 1, characterized in that: The preset temperature T3 of step (3) is 325-400°C.

5. The non-isothermal treatment method for improving the annealing softening resistance and yield ratio of aluminum alloy according to claim 1, characterized in that: The cooling rate of step (4) is 0.5 to 5°C / min.

6. The non-isothermal treatment method for improving the annealing softening resistance and yield ratio of aluminum alloy according to claim 1, characterized in that: The total time of step (1), step (2) and step (3) is 120 to 150 minutes.