High-strength biodegradable Zn-Mn alloy under synergistic effect of GPa-level high pressure and cold rolling and preparation method of high-strength biodegradable Zn-Mn alloy

Through the preparation method of GPa-level high pressure and cold rolling synergistically, the mechanical properties of Zn-Mn alloy are improved, the problem of insufficient strength is solved, the mechanical requirements of human implanted devices are met, and the degradation uniformity of the material is improved and Corrosion resistance.

CN118932263APending Publication Date: 2024-11-12XIANGTAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410982236.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing Zn-Mn alloys are insufficient in strength and cannot meet the mechanical requirements of human implantation devices. The sample size of high-pressure synthesized is too small to be applied to different implantation sites.

Method used

Using the preparation method of synergistic effect of GPa-level high pressure and cold rolling, Zn-Mn alloy with a Mn content of 0.5 to 1.5% is prepared by homogenizing annealing, GPa-level high pressure synthesis and multi-pass cold rolling treatment, and its tensile yield is improved. Strength, ultimate tensile strength and elongation.

Benefits of technology

It significantly improves the mechanical properties of Zn-Mn alloy, with tensile yield strength of 190~300MPa, ultimate tensile strength of 230~330MPa, and elongation of 35~65%, meeting the mechanical properties requirements of human implanted materials and improving The degradation uniformity and corrosion resistance of the material are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932263A_ABST
    Figure CN118932263A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of biomedical metal materials, and particularly discloses a preparation method of a high-strength biodegradable Zn-Mn alloy under the synergistic effect of GPa-level high pressure and cold rolling, and the preparation method comprises the following steps: carrying out homogenizing annealing on a Zn-Mn alloy cast ingot to obtain an annealed part; the annealed part is subjected to GPa-level high-pressure synthesis, the GPa-level high-pressure synthesis technological parameters are as follows: the pressure is 3-5 GPa, the synthesis temperature is 700-900 DEG C, the heating rate is 100-300 DEG C / min, and the temperature and pressure are kept for 30-60 min, and a high-pressure part is obtained; and the high-pressure part is subjected to multi-pass cold rolling, the rolling reduction of each pass is 0.8-2 mm, the final deformation is 80-85%, and a biological Zn-Mn alloy finished product is obtained. By adjusting and optimizing the preparation process, the biodegradable Zn-Mn alloy with excellent mechanical properties is prepared, has high mechanical property reliability, meets the mechanical property requirements of human body implant materials, and is beneficial to the application of the Zn-Mn alloy in the field of medical implant medical instruments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of biomedical metal material preparation, and in particular to a high-strength biodegradable Zn-Mn alloy under the synergistic effect of GPa-level high pressure and cold rolling and a preparation method thereof. Background Art

[0002] With the rapid development of society, the aging population is becoming more and more serious, which has put forward a huge demand for the required medical resources. Compared with traditional biometals, biodegradable metal implants do not require secondary surgery to remove, which reduces the physical pain and economic pressure of patients. Biodegradable metals are mainly divided into three categories: magnesium-based (Mg), zinc-based (Zn) and iron-based (Fe) materials. However, the degradation rate of magnesium-based materials is very fast, it is difficult to maintain mechanical integrity in the body, premature failure and hydrogen evolution reaction during the degradation process release a large amount of hydrogen, which hinders their clinical application. The slow degradation of iron-based materials in the body hinders the self-healing of human bones. Zinc-based biodegradable materials have a moderate degradation rate and acceptable biocompatibility and are considered to be potential biodegradable materials. More importantly, zinc is one of the essential trace elements in the human body. As a component element of various enzymes, it is closely related to the development of the body, the immune system and reproductive inheritance. In addition, Zn ions also have antibacterial activity, indicating that the controlled release of Zn ions can lead to antibacterial activity against postoperative inflammation and infection.

[0003] Pure zinc cannot meet the mechanical requirements of clinical applications because of its poor mechanical properties and tensile yield strength of less than 50MPa. Therefore, alloying and thermoplastic deformation (such as hot rolling and hot extrusion) are usually used to eliminate the brittleness of zinc and improve its yield strength. At present, the selection of alloying elements mainly focuses on Mn, Li, Mg, Cu, Ag, etc. Due to the influence of solid solution strengthening and precipitation hardening, solid solubility is an important factor in selecting alloying elements to strengthen metals. Mn has a significant solid solubility in Zn. In the Zn-Mn phase diagram, the maximum solid solubility of Mn at 400°C can reach 0.8wt.%; in addition, Mn plays an important role in organisms and is a synergistic factor of many enzymes. It has the functions of promoting lipid metabolism, participating in hematopoiesis, and enhancing immunity. However, the strength of Zn-Mn alloy is much lower than that of other binary alloys. The strength of Zn-Mn alloy prepared by most preparation processes is generally lower than 200MPa, which cannot meet the requirements of human implantation (the mechanical requirements of vascular stents and bone implants are ultimate tensile strength (UTS)>300MPa, tensile yield strength (YS)>200MPa, and plasticity (EL)>15-18%). Chinese patent publication number CN 107177754A discloses a high plasticity and biodegradable Zn-Mn zinc alloy and a preparation method thereof. The Zn-Mn zinc alloy is obtained by alloy melting and casting-homogenization annealing-hot rolling-cold rolling preparation process. The Zn-Mn zinc alloy has high plasticity, but low yield strength and tensile strength.

[0004] GPa-level high-pressure synthesis technology has been widely studied and applied as a new type of special processing and preparation technology to improve the mechanical properties of alloys. Under the action of high pressure, the pressure reduces the nucleation activation energy and increases the nucleation rate, while inhibiting atomic diffusion, thereby increasing the diffusion activation energy, thereby increasing the activation energy of crystal growth and reducing the crystal growth rate. However, the inventors of this application found in their research that GPa-level high-pressure synthesis technology can improve the strength of Zn-Mn alloys, but the improvement effect is limited and cannot meet the mechanical requirements of implantable devices; in order to meet the requirements of human implantation, its strength needs to be further improved. In addition, the sample size of high-pressure synthesis is too small to be applied to the size of different implant sites. Summary of the invention

[0005] In view of the above shortcomings, the present invention provides a method for preparing a high-strength biodegradable Zn-Mn alloy under the synergistic effect of GPa-level high pressure and cold rolling. The prepared Zn-Mn alloy has excellent mechanical properties. The specific technical scheme is as follows:

[0006] A method for preparing a high-strength biodegradable Zn-Mn alloy under the synergistic effect of GPa-level high pressure and cold rolling, wherein the Mn content of the Zn-Mn alloy is 0.5-1.5% by mass and the balance is Zn; the preparation method comprises the following steps:

[0007] (1) performing homogenization annealing on a Zn-Mn alloy ingot to obtain an annealed part;

[0008] (2) subjecting the annealed part to GPa-level high-pressure synthesis, wherein the process parameters of the GPa-level high-pressure synthesis are: pressure of 3 GPa to 5 GPa, synthesis temperature of 700 to 900°C, heating rate of 100 to 300°C / min, and heat and pressure maintenance for 30 to 60 min to obtain a high-pressure part;

[0009] (3) The high-pressure component is subjected to multiple cold rolling passes, with each pass having a reduction of 0.8 to 2 mm and a final deformation of 80 to 85%, to obtain a biodegradable Zn-Mn alloy product.

[0010] Preferably, in the above preparation method, the Mn content in the Zn-Mn alloy is 0.8-1.5%, and the balance is Zn.

[0011] Preferably, in the above-mentioned preparation method, in the step (1), the homogenization annealing temperature is 250-350° C., and the holding time is 3-10 hours.

[0012] Preferably, in the above-mentioned preparation method, in the step (2), after heat preservation and pressure preservation, water cooling to room temperature is performed, and the cooling rate is 10 to 50°C / s.

[0013] Preferably, in the above-mentioned preparation method, the step (2) is specifically as follows: using a wire cutting machine to cut a cylindrical sample with a diameter of 10 mm and a height of 18 mm from the annealed piece, and grinding the surface with sandpaper until it is smooth; placing the cylindrical sample into a boron nitride sleeve, a graphite sleeve, and talc in sequence, using molybdenum sheets and steel caps on both sides for conductive packaging, assembling into a set, and then placing the assembled set into a six-sided top press, setting the pressure to 3GPa~5GPa, and setting the heating temperature to 700~900℃ according to the Clausius-Clapeyren equation and the melting point of the Zn-Mn alloy; increasing the pressure of the six-sided top press to a preset pressure, and then raising the temperature to a preset temperature at a rate of 100~300℃ / min, keeping the temperature and pressure for 30~60min, and finally cooling it to room temperature by water cooling, and releasing the pressure to obtain a high-pressure sample.

[0014] Preferably, in the above-mentioned preparation method, the Zn-Mn alloy ingot is prepared by: respectively mixing Zn and Mn according to mass percentage, placing Zn and Mn in a vacuum induction melting furnace, melting at 650°C for 10 minutes under argon protection, then pouring into a graphite mold, and obtaining the Zn-Mn alloy ingot after cooling to room temperature.

[0015] On the other hand, the present invention also provides a high-strength biodegradable Zn-Mn alloy prepared by the above preparation method.

[0016] Preferably, in the above Zn-Mn alloy, the Zn-Mn alloy has a tensile yield strength of 190 to 300 MPa, an ultimate tensile strength of 230 MPa to 330 MPa, and an elongation of 35 to 65%.

[0017] On the other hand, the present invention also provides the use of the above Zn-Mn alloy in biodegradable medical implant materials.

[0018] Preferably, in the above application, the biodegradable medical implant material is at least one of a degradable vascular stent and a degradable orthopedic implant.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. In the preparation method of the present invention, a biodegradable Zn-Mn alloy with excellent mechanical properties is prepared by optimizing and effectively controlling the preparation process. The Zn-Mn alloy has a tensile yield strength of 190 to 300 MPa, an ultimate tensile strength of 230 MPa to 330 MPa, and an elongation of 35 to 65%. It has high mechanical property reliability, meets the mechanical property requirements of human implant materials, and is conducive to the application of Zn-Mn alloy in the field of medical implant medical devices.

[0021] 2. In the preparation method of the present invention, the mechanical properties of the Zn-Mn alloy are significantly improved through the synergistic effect of high-pressure treatment and cold rolling treatment, and the Mn atoms are dissolved into the Zn matrix. The disappearance of the second phase eliminates the micro-electrochemical corrosion of the alloy, improves the degradation uniformity of the material, and exhibits a more positive corrosion potential and a lower corrosion current density and corrosion rate. It has a slower degradation rate and is not prone to premature failure when implanted as a degradable material. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0023] Figure 1 XRD patterns of Zn-Mn alloys prepared in Examples 1 to 3 and Comparative Examples 1 to 3 of the present invention;

[0024] Figure 2 Electrochemical corrosion polarization curves of Zn-Mn alloys prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 to 3 in Hanks solution. DETAILED DESCRIPTION

[0025] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments. Unless otherwise defined, all professional terms used hereinafter have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the protection scope of the present invention. Unless otherwise specifically stated, various raw materials, reagents, instruments and equipment used in the present invention, etc. can be purchased from the market or can be prepared by existing methods.

[0026] Example 1

[0027] A method for preparing a high-strength biodegradable Zn-Mn alloy under the synergistic effect of GPa-level high pressure and cold rolling, comprising the following steps:

[0028] (1) Using a Zn ingot with a purity of 99.99% and a pure Mn with a purity of 99.99% as raw materials, and weighing and mixing the two elements in a binary Zn-Mn alloy composition in a mass ratio of 99.5:0.5, Zn and Mn are placed in a vacuum induction melting furnace, smelted at 650° C. for 10 min under argon protection, and then poured into a graphite mold, and cooled to room temperature to obtain a Zn-Mn alloy ingot;

[0029] (2) homogenizing the Zn-Mn alloy ingot and keeping it at 300° C. for 5 h; after the annealing, the ingot is taken out of the heating furnace and cooled in air to obtain an annealed part;

[0030] (3) Using a wire cutting machine to cut a cylindrical sample with a diameter of 10 mm and a height of 18 mm from the annealed piece, and polishing the surface with sandpaper until it is smooth; placing the cylindrical sample into a boron nitride sleeve, a graphite sleeve, and pyrophyllite in turn, using molybdenum sheets and steel caps on both sides for conductive packaging, assembling into a set, and then placing the assembled set into a six-sided top press for high-pressure solidification, setting the pressure to 5 GPa, and setting the heating temperature to 800 degrees Celsius according to the Clausius-Clapeyren equation and the melting point of the Zn-Mn alloy; increasing the pressure of the six-sided top press to a preset pressure, and then increasing the temperature to a preset temperature at a rate of 300°C / min, stopping heating after keeping the temperature and pressure for 60 minutes, and rapidly cooling to room temperature at a rate of 10-50°C / s with the help of a water cooling device, and releasing the pressure to obtain a high-pressure part;

[0031] (4) The high-pressure parts were prepared into 7.5 mm thick plates by wire cutting machine for rolling. Four cold rolling passes were performed with reductions of 1.5 mm, 2 mm, 2 mm, and 0.8 mm, respectively. The plates were rolled to 1.2 mm thick (84% deformation), which was a high-strength biodegradable Zn-Mn alloy, denoted as HPS-CR Zn-0.5Mn.

[0032] Example 2

[0033] A method for preparing a high-strength biodegradable Zn-Mn alloy under the synergistic effect of GPa-level high pressure and cold rolling, comprising the following steps:

[0034] (1) Using a Zn ingot with a purity of 99.99% and a pure Mn with a purity of 99.99% as raw materials, and weighing and mixing the ingredients according to the mass ratio of the two elements in the binary Zn-Mn alloy composition of 99.0:1.0, Zn and Mn are placed in a vacuum induction melting furnace, smelted at 650° C. for 10 minutes under argon protection, and then poured into a graphite mold, and cooled to room temperature to obtain a Zn-Mn alloy ingot;

[0035] (2) homogenizing the Zn-Mn alloy ingot and keeping it at 300° C. for 5 h; after the annealing, the ingot is taken out of the heating furnace and cooled in air to obtain an annealed part;

[0036] (3) Using a wire cutting machine to cut a cylindrical sample with a diameter of 10 mm and a height of 18 mm from the annealed piece, and polishing the surface with sandpaper until it is smooth; placing the cylindrical sample into a boron nitride sleeve, a graphite sleeve, and pyrophyllite in turn, using molybdenum sheets and steel caps on both sides for conductive packaging, assembling into a set, and then placing the assembled set into a six-sided top press for high-pressure solidification, setting the pressure to 5 GPa, and setting the heating temperature to 800 degrees Celsius according to the Clausius-Clapeyren equation and the melting point of the Zn-Mn alloy; increasing the pressure of the six-sided top press to a preset pressure, and then increasing the temperature to a preset temperature at a rate of 300°C / min, stopping heating after keeping the temperature and pressure for 60 minutes, and rapidly cooling to room temperature at a rate of 10-50°C / s with the help of a water cooling device, and releasing the pressure to obtain a high-pressure part;

[0037] (4) The high-pressure parts were prepared into 7.5 mm thick plates by wire cutting machine for rolling. Four cold rolling passes were performed with reductions of 1.5 mm, 2 mm, 2 mm, and 0.8 mm, respectively. The plates were rolled to 1.2 mm thick (84% deformation), which was a high-strength biodegradable Zn-Mn alloy, denoted as HPS-CR Zn-1.0Mn.

[0038] Example 3

[0039] A method for preparing a high-strength biodegradable Zn-Mn alloy under the synergistic effect of GPa-level high pressure and cold rolling, comprising the following steps:

[0040] (1) Using a Zn ingot with a purity of 99.99% and a pure Mn with a purity of 99.99% as raw materials, and weighing and mixing the two elements in a binary Zn-Mn alloy composition in a mass ratio of 98.5:1.5, Zn and Mn are placed in a vacuum induction melting furnace, smelted at 650° C. for 10 min under argon protection, and then poured into a graphite mold, and cooled to room temperature to obtain a Zn-Mn alloy ingot;

[0041] (2) homogenizing the Zn-Mn alloy ingot and keeping it at 300° C. for 5 h; after the annealing, the ingot is taken out of the heating furnace and cooled in air to obtain an annealed part;

[0042] (3) Using a wire cutting machine to cut a cylindrical sample with a diameter of 10 mm and a height of 18 mm from the annealed piece, and polishing the surface with sandpaper until it is smooth; placing the cylindrical sample into a boron nitride sleeve, a graphite sleeve, and pyrophyllite in turn, using molybdenum sheets and steel caps on both sides for conductive packaging, assembling into a set, and then placing the assembled set into a six-sided top press for high-pressure solidification, setting the pressure to 5 GPa, and setting the heating temperature to 800 degrees Celsius according to the Clausius-Clapeyren equation and the melting point of the Zn-Mn alloy; increasing the pressure of the six-sided top press to a preset pressure, and then increasing the temperature to a preset temperature at a rate of 300°C / min, stopping heating after keeping the temperature and pressure for 60 minutes, and rapidly cooling to room temperature at a rate of 10-50°C / s with the help of a water cooling device, and releasing the pressure to obtain a high-pressure part;

[0043] (4) The high-pressure parts were prepared by wire cutting machine to form 7.5 mm thick plates for rolling. Four cold rolling passes were performed with reductions of 1.5 mm, 2 mm, 2 mm, and 0.8 mm, respectively. The plates were rolled to 1.2 mm thick (84% deformation), which was a high-strength biodegradable Zn-Mn alloy, denoted as HPS-CR Zn-1.5Mn.

[0044] Comparative Example 1

[0045] A method for preparing a Zn-Mn alloy comprises the following steps:

[0046] (1) Using a Zn ingot with a purity of 99.99% and a pure Mn with a purity of 99.99% as raw materials, and weighing and mixing the two elements in a binary Zn-Mn alloy composition in a mass ratio of 99.5:0.5, Zn and Mn are placed in a vacuum induction melting furnace, smelted at 650° C. for 10 min under argon protection, and then poured into a graphite mold, and cooled to room temperature to obtain a Zn-Mn alloy ingot;

[0047] (2) homogenizing the Zn-Mn alloy ingot and keeping it at 300° C. for 5 h; after the annealing, the ingot is taken out of the heating furnace and cooled in air to obtain an annealed part;

[0048] (3) The annealed parts were prepared into 7.5 mm thick plates by wire cutting for rolling. Four cold rolling passes were performed with reductions of 1.5 mm, 2 mm, 2 mm, and 0.8 mm, respectively. The plates were rolled to 1.2 mm thick (84% deformation), which was Zn-Mn alloy and recorded as CR Zn-0.5Mn.

[0049] Comparative Example 2

[0050] A method for preparing a Zn-Mn alloy comprises the following steps:

[0051] (1) Using a Zn ingot with a purity of 99.99% and a pure Mn with a purity of 99.99% as raw materials, and weighing and mixing the ingredients according to the mass ratio of the two elements in the binary Zn-Mn alloy composition of 99.0:1.0, Zn and Mn are placed in a vacuum induction melting furnace, smelted at 650° C. for 10 minutes under argon protection, and then poured into a graphite mold, and cooled to room temperature to obtain a Zn-Mn alloy ingot;

[0052] (2) homogenizing the Zn-Mn alloy ingot and keeping it at 300° C. for 5 h; after the annealing, the ingot is taken out of the heating furnace and cooled in air to obtain an annealed part;

[0053] (3) The annealed piece was prepared into a 7.5 mm thick plate by wire cutting for rolling. Four cold rolling passes were performed with reductions of 1.5 mm, 2 mm, 2 mm, and 0.8 mm, respectively. The plate was rolled to a thickness of 1.2 mm (84% deformation), which is a Zn-Mn alloy, denoted as CR Zn-1.0Mn.

[0054] Comparative Example 3

[0055] A method for preparing a Zn-Mn alloy comprises the following steps:

[0056] (1) Using a Zn ingot with a purity of 99.99% and a pure Mn with a purity of 99.99% as raw materials, and weighing and mixing the two elements in a binary Zn-Mn alloy composition in a mass ratio of 98.5:1.5, Zn and Mn are placed in a vacuum induction melting furnace, smelted at 650° C. for 10 min under argon protection, and then poured into a graphite mold, and cooled to room temperature to obtain a Zn-Mn alloy ingot;

[0057] (2) homogenizing the Zn-Mn alloy ingot and keeping it at 300° C. for 5 h; after the annealing, the ingot is taken out of the heating furnace and cooled in air to obtain an annealed part;

[0058] (3) The annealed parts were prepared into 7.5 mm thick plates by wire cutting for rolling. Four cold rolling passes were performed with reductions of 1.5 mm, 2 mm, 2 mm, and 0.8 mm, respectively. The plates were rolled to 1.2 mm thick (84% deformation), which was Zn-Mn alloy and was recorded as CR Zn-1.5Mn.

[0059] The XRD patterns of the Zn-Mn alloys prepared in Examples 1 to 3 and Comparative Examples 1 to 3 are shown in Figure 1 The electrochemical corrosion polarization curve in Hanks solution is shown in Figure 2 .Depend on Figure 1 and Figure 2 It can be seen that after high pressure and cold rolling treatment, the peak position of the diffraction peak in the Zn-Mn alloy tends to shift to a low angle, and the diffraction peak of the second phase disappears, indicating that the Mn atoms after high pressure and cold rolling treatment are dissolved into the Zn matrix. The disappearance of the second phase eliminates the micro-electrochemical corrosion of the alloy, improves the degradation uniformity of the material, and exhibits a more positive corrosion potential and a lower corrosion current density and corrosion rate.

[0060] The mechanical properties of the high-pressure solidified and annealed Zn-Mn alloys prepared in Examples 1 to 3 are compared in Table 1. As can be seen from Table 1, the mechanical properties of the alloy after high-pressure treatment are greatly improved, but its yield strength and tensile strength are both lower than 200 MPa, which does not meet the mechanical property requirements of implantable devices.

[0061] Table 1 Mechanical properties of high pressure solidified and cast Zn-Mn alloys prepared in Examples 1 to 3

[0062]

[0063] Table 2 shows the mechanical properties of the Zn-Mn alloys prepared in Examples 1 to 3 and Comparative Examples 1 to 3. It can be seen from the table that the mechanical properties of the alloys obtained by combining high pressure treatment and cold rolling treatment are significantly improved compared with those of the Zn-Mn alloys directly cold rolled and solidified under high pressure. The Zn-1.5Mn alloy under the synergistic effect of high pressure and cold rolling has a tensile yield strength of 300 MPa, an ultimate tensile strength of 330 MPa, and an elongation of 35%. The tensile yield strength is increased by 140.1%, and the ultimate tensile strength is increased by 107.3%. It has higher mechanical property reliability and meets the mechanical requirements of implantable devices.

[0064] Table 2 Mechanical properties of Zn-Mn alloys prepared in Examples 1 to 3 and Comparative Examples 1 to 3

[0065]

[0066]

[0067] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.

Claims

1. A method for preparing a high-strength biodegradable Zn-Mn alloy under the synergistic effect of GPa-level high pressure and cold rolling, characterized in that: In terms of mass percentage, the Mn content in the Zn-Mn alloy is 0.5-1.5%, and the balance is Zn. The preparation method comprises the following steps: (1) performing homogenization annealing on a Zn-Mn alloy ingot to obtain an annealed part; (2) subjecting the annealed part to GPa-level high-pressure synthesis, wherein the process parameters of the GPa-level high-pressure synthesis are: pressure of 3 GPa to 5 GPa, synthesis temperature of 700 to 900°C, heating rate of 100 to 300°C / min, and heat and pressure maintenance for 30 to 60 min to obtain a high-pressure part; (3) The high-pressure component is subjected to multiple cold rolling passes, with each pass having a reduction of 0.8 to 2 mm and a final deformation of 80 to 85%, to obtain a biodegradable Zn-Mn alloy product.

2. The preparation method according to claim 1, characterized in that: The Zn-Mn alloy contains 0.8-1.5% Mn and the balance is Zn.

3. The preparation method according to claim 1, characterized in that: In the step (1), the homogenization annealing temperature is 250-350° C., and the holding time is 3-10 hours.

4. The preparation method according to claim 1, characterized in that: In the step (2), the mixture is kept warm and pressure maintained and then cooled to room temperature with water.

5. The preparation method according to claim 1, characterized in that: The Zn-Mn alloy ingot is prepared by respectively mixing Zn and Mn according to mass percentage, placing Zn and Mn in a vacuum induction melting furnace, melting at 650° C. for 10 minutes under argon protection, then pouring into a graphite mold, and obtaining the Zn-Mn alloy ingot after cooling to room temperature.

6. A high-strength biodegradable Zn-Mn alloy prepared by the preparation method according to any one of claims 1 to 5.

7. The Zn-Mn alloy according to claim 6, characterized in that: The Zn-Mn alloy has a tensile yield strength of 190-300 MPa, an ultimate tensile strength of 230 MPa-330 MPa, and an elongation of 35-65%.

8. Use of the Zn-Mn alloy as claimed in claim 6 or 7 in biodegradable medical implant materials.