Hydrophobic / chromium-rich corrosion-resistant composite coating as well as preparation method and application thereof
By coating slurry containing chromium powder, nickel powder, iron powder and rare earth compounds on the surface of the boiler pipe and spraying superhydrophobic materials, a hydrophobic/chromium-rich corrosion-resistant composite coating is formed, and the oxidation and corrosion-resistant problem under high temperature and high pressure is solved, and the oxidation and corrosion resistance problem is achieved. The corrosion resistance, wear resistance and hydrophobic properties of the pipeline extend the service life of the pipeline.
Patent Information
- Application Number
- CN202410975831.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art cannot effectively solve the oxidative corrosion problem of boiler pipelines under high temperature and high pressure conditions, resulting in safety hazards such as short pipeline life and regular oxide treatment.
The preparation method of hydrophobic/chromium-rich corrosion-resistant composite coating is adopted. After preheating treatment, the slurry containing chromium powder, nickel powder, iron powder and rare earth compounds is coated on the surface of the workpiece, and superhydrophobic material is sprayed on the surface to form a Coatings with corrosion resistance, wear resistance and hydrophobic properties.
This method not only improves the corrosion resistance and oxidation resistance of the pipeline, but also prevents water vapor from staying and avoids metal oxidation corrosion, thereby extending the service life of the pipeline and improving the overall performance.
Smart Images

Figure CN118932332A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of material surface coatings, and in particular relates to a hydrophobic / chromium-rich corrosion-resistant composite coating and a preparation method and application thereof. Background Art
[0002] Thermal corrosion of the inner surface of boiler pipes has always been one of the factors restricting thermal power generation. Especially at the current stage, the working conditions of thermal power generation are developing towards higher steam temperature and pressure. It is urgent to improve the thermal corrosion resistance of the inner surface of pipes.
[0003] Pipeline corrosion problems mainly consist of two parts: one is the corrosion caused by gas, and the other is the metal oxidation corrosion caused by water vapor. By building a corrosion-resistant coating on the surface of the pipe, problems such as short pipeline life and regular treatment of oxides can be solved, and dangerous events such as pipeline bursts can be avoided.
[0004] At present, the most common anti-corrosion technology is the technology of infiltrating corrosion-resistant metals on the surface of alloys, such as Al, Si, Cr, etc.; a corrosion-resistant coating is formed on the surface of the alloy by infiltrating Cr, and there are many methods for preparing Cr-rich coatings, usually including powder embedding method, vapor deposition method and liquid phase method. The liquid phase method usually puts Cr powder into molten salt and forms a Cr-infiltrated layer by high-temperature insulation. However, the molten salt is easy to volatilize at high temperatures in this method, causing damage to the workpiece and the environment. The slurry method is to obtain a coating by directly applying or spraying the slurry to the surface of the workpiece and then sintering it at high temperature. This method obtains a coating with excellent corrosion resistance and good adhesion. Compared with other Cr-infiltrating methods, this method is simple to operate and suitable for large-scale industrial production.
[0005] However, according to the saturated vapor pressure of water, it is found that liquid water can still exist in the pipeline under high temperature and high pressure conditions. The above anti-corrosion methods can only delay pipeline corrosion to a certain extent, and still cannot solve the problem of pipeline oxidation corrosion from the root. Summary of the invention
[0006] The present disclosure aims to solve at least one of the technical problems existing in the prior art and to provide a hydrophobic / chromium-rich corrosion-resistant composite coating and a preparation method and application thereof.
[0007] In one aspect of the present disclosure, a method for preparing a hydrophobic / chromium-rich corrosion-resistant composite coating is provided, the preparation method comprising:
[0008] Preheating the workpiece;
[0009] The coating slurry is applied to the surface of the workpiece after preheating treatment, and after drying, solidification and sintering treatment, a chromium-rich corrosion-resistant coating is obtained on the surface of the workpiece; the coating slurry includes a solid phase component and a liquid phase component; wherein the solid phase component includes chromium powder, nickel powder, iron powder and rare earth compounds; the liquid phase component includes Al(H2PO4)3, water glass, ammonium halide, polyvinyl alcohol and Cr2O3;
[0010] A layer of super hydrophobic material is sprayed on the surface of the chromium-rich corrosion-resistant coating, and a hydrophobic / chromium-rich corrosion-resistant composite coating is obtained through curing.
[0011] Optionally, the solid-liquid ratio of the solid phase component to the liquid phase component is 10:(1-5).
[0012] Optionally, the content of the chromium powder is 40-80%;
[0013] The content of the nickel powder is 5-30%;
[0014] The content of the iron powder is 2-20%;
[0015] The content of the rare earth compound is 5-45%.
[0016] Optionally, the content of Al(H2PO4)3 is 10-30%;
[0017] The content of water glass is 15-25%;
[0018] The content of the ammonium halide is 5 to 10%;
[0019] The content of polyvinyl alcohol is 10-35%;
[0020] The content of Cr2O3 is 10-30%.
[0021] Optionally, the rare earth compound is a rare earth oxide or a rare earth chloride; and / or,
[0022] The ammonium halide is ammonium bromide or ammonium iodide.
[0023] Optionally, a layer of super hydrophobic material is sprayed on the surface of the chromium-rich corrosion-resistant coating, and a hydrophobic / chromium-rich corrosion-resistant composite coating is obtained by curing, comprising:
[0024] Anhydrous ethanol, HDTMS and nano-alumina particles are mixed to prepare a suspension, and HDTMS-modified super-hydrophobic Al2O3 nanoparticles are obtained through stirring, centrifugation and drying.
[0025] Epoxy resin, polydimethylsiloxane, epoxy resin curing agent, and Al2O3 nanoparticles treated with HDTMS hydrophobicity are dissolved in xylene to prepare a suspension, which is sprayed on the surface of the chromium-rich corrosion-resistant coating, and a super-hydrophobic / chromium-rich corrosion-resistant composite coating is obtained after curing.
[0026] Optionally, the workpiece is preheated at a temperature of 150 to 220° C. for a time of 30 to 60 minutes; and / or,
[0027] Under the protection of inert gas, the sintering temperature is 980-1150°C and the time is 8-30 minutes.
[0028] Optionally, the thickness of the chromium-rich corrosion-resistant coating is 5 to 50 μm; and / or,
[0029] The thickness of the hydrophobic / chromium-rich corrosion-resistant composite coating is 13-64 μm.
[0030] In another aspect of the present disclosure, a hydrophobic / chromium-rich corrosion-resistant composite coating is provided, which is prepared according to the preparation method described above.
[0031] Another aspect of the present disclosure provides an application of a hydrophobic / chromium-rich corrosion-resistant composite coating, wherein the hydrophobic / chromium-rich corrosion-resistant composite coating described above is applied to the inner surface of a boiler pipe.
[0032] The present disclosure proposes a hydrophobic / chromium-rich corrosion-resistant composite coating and its preparation method and application. The preparation method includes: preheating the workpiece; coating the coating slurry on the surface of the workpiece after preheating, drying, curing and sintering to obtain a chromium-rich corrosion-resistant coating on the surface of the workpiece; the coating slurry includes solid phase components and liquid phase components; wherein the solid phase components include chromium powder, nickel powder, iron powder and rare earth compounds; the liquid phase components include Al(H2PO4)3, water glass, ammonium halide, polyvinyl alcohol and Cr2O3; spraying a layer of super-hydrophobic material on the surface of the chromium-rich corrosion-resistant coating, and curing to obtain a hydrophobic / chromium-rich corrosion-resistant composite coating. The method makes the workpiece have corrosion resistance and wear resistance by chromizing and super-hydrophobic treatment of the workpiece, and also has hydrophobic characteristics, so that the water vapor in the pipeline cannot stay on the inner wall of the pipeline, which can avoid corrosion of the inner wall of the pipeline, thereby improving the comprehensive performance of the pipeline and extending its service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The present invention is a flowchart of a method for preparing a hydrophobic / chromium-rich corrosion-resistant composite coating according to an embodiment of the present invention. DETAILED DESCRIPTION
[0034] In order to enable those skilled in the art to better understand the technical solution of the present disclosure, the present disclosure is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present disclosure.
[0035] like Figure 1 As shown, in one aspect of the present disclosure, a method S100 for preparing a hydrophobic / chromium-rich corrosion-resistant composite coating is provided, which specifically comprises the following steps S110 to S130:
[0036] S110, preheating the workpiece.
[0037] Specifically, the workpiece is preheated at a temperature of 150 to 220° C. for 30 to 60 minutes.
[0038] In this embodiment, the preheating treatment can optimize the organizational structure of the metal workpiece, eliminate residual stress, reduce deformation of the workpiece, improve surface quality, and increase the temperature of the workpiece, which is beneficial for subsequent coating of chromizing slurry on its surface.
[0039] It should be understood that the workpiece can also be cleaned before preheating, for example: using alcohol or acetone to clean oil stains, dust, etc. on the surface of the pipe, and using a steel brush to remove the surface oxide scale to increase the specific surface area of the workpiece, enhance the subsequent metal powder penetration effect, and increase the adhesion of the coating.
[0040] S120, coating the coating slurry on the surface of the workpiece after preheating treatment, drying, curing and sintering to obtain a chromium-rich corrosion-resistant coating on the surface of the workpiece.
[0041] In this embodiment, the coating slurry includes a solid phase component and a liquid phase component; wherein the solid phase component includes chromium powder, nickel powder, iron powder and rare earth compound; and the liquid phase component includes Al(H2PO4)3, water glass, ammonium halide, polyvinyl alcohol and Cr2O3. By mixing the solid phase component and the liquid phase component in a certain proportion to form a slurry, it is helpful for each metal powder to be coated on the surface of the workpiece to form a corrosion-resistant coating.
[0042] In some preferred embodiments, the solid-liquid ratio (g:mL) of the solid phase component to the liquid phase component is 10:(1-5), for example, the two components are mixed in a ratio of 10:1, 10:2, 10:3, 10:4, 10:5, etc.
[0043] It should be noted that the present embodiment does not specifically limit the mixing form of the solid phase component and the liquid phase component. The solid phase component can be directly added to the liquid phase component, or the liquid phase component can be injected into the solid phase component for mixing. Of course, the powders in the solid phase component can also be mixed in advance, for example, each solid phase component is ball milled in a star ball mill at a speed of 350 to 400 r / min for 6 to 24 hours to pre-mix the solid phase components, and then the mixed solid phase components are mixed with the liquid phase components.
[0044] In some preferred embodiments, the content of chromium powder is 40-80%, for example, 40%, 50%, 60%, 70%, 80%; the content of nickel powder is 5-30%, for example, 5%, 10%, 15%, 20%, 25%, 30%; the content of iron powder is 2-20%, for example, 2%, 7%, 10%, 15%, 17%, 20%; the content of rare earth compound is 5-45%, for example, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%.
[0045] As a further preferred embodiment, the rare earth compound is a rare earth oxide, such as samarium oxide, europium oxide, yttrium oxide, etc. Of course, the rare earth compound can also be a rare earth chloride, such as lanthanum chloride, etc.
[0046] In the solid phase components of this embodiment, rare earth atoms are provided by adding oxides and chlorides of rare earth elements. During the sintering process, the oxides or chlorides of rare earth elements are segregated at the grain boundaries, playing the role of pinning the grain boundaries, which can refine the coating grains; at the same time, it can prevent Cr atoms from diffusing deeper into the substrate, causing the coating to grow outward, increasing the thickness of the coating and the Cr element concentration in the coating; during the service process, they are segregated at the grain boundaries of the oxide film, thereby inhibiting the Cr 3+ The rapid "short-circuit diffusion" along the grain boundaries makes the oxidation mechanism of the coating changed from Cr 3+ Diffusion outward mainly transforms into O 2- Diffusion inward, this internally grown oxide film is tightly bonded to the substrate, improving the oxide film's resistance to spalling and thereby enhancing the coating's corrosion resistance.
[0047] Furthermore, in the solid phase components of this embodiment, a small amount of iron and nickel are added mainly to increase the chromizing speed and reduce the chromizing temperature; chromium forms solid solutions with iron and nickel elements respectively. Compared with a single chromizing coating, chromium-iron-nickel co-diffusion can significantly improve the wear resistance and corrosion resistance of the chromized layer.
[0048] In other preferred embodiments, the content of Al(H2PO4)3 is 10-30%, for example, 10%, 15%, 20%, 25%, 30%; the content of water glass is 15-25%, for example, 15%, 20%, 25%; the content of ammonium halide is 5-10%, for example, 5%, 7%, 10%; the content of polyvinyl alcohol is 10-35%, for example, 10%, 20%, 25%, 30%, 35%; the content of Cr2O3 is 10-30%, for example, 10%, 15%, 20%, 25%, 30%.
[0049] As a further preferred embodiment, the ammonium halide is ammonium bromide or ammonium iodide.
[0050] In the liquid phase component of the present embodiment, the synergistic effect of the liquid phase component and the solid phase component can realize a one-time coating process to prepare a coating of a desired thickness, and the coating has a smooth surface, a uniform and dense interior, and good corrosion resistance.
[0051] Furthermore, in the liquid phase component of the present embodiment, Al(H2PO4)3 acts as a binder, and has a high bonding strength with the metal substrate, and a single coating treatment can achieve the required thickness for preparing the coating; at the same time, the component has good high-temperature toughness and is not prone to cracking during the curing and drying process.
[0052] Furthermore, in the liquid phase component of the present embodiment, the binder is modified by adding water glass and polyvinyl alcohol, so as to further increase the high temperature toughness of Al(H2PO4)3 and its adhesion to the metal substrate, and Al(H2PO4)3, as an inorganic binder, can directly volatilize during the drying of the slurry, and will not generate gas due to decomposition during the sintering process, resulting in the formation of pores inside the coating. In other words, the polyvinyl alcohol of the present embodiment is a substance that can improve the high temperature toughness and bonding strength of Al(H2PO4)3.
[0053] Furthermore, in the liquid phase component of the present embodiment, NH4I or NH4Br acts as a penetration enhancer to promote the generation of active chromium atoms and nickel atoms.
[0054] Furthermore, in the liquid phase component of the present embodiment, Cr2O3 acts as a curing agent to dehydrate and condense the acid phosphate in the binder, which can effectively reduce the curing and film-forming temperature of the slurry. In addition, adding an appropriate amount of Cr2O3 can also improve the curing and film-forming performance of Al(H2PO4)3, so that the surface of the coating layer after drying and curing is smooth and flat, and the interior is uniform and dense.
[0055] It should be further explained that the present embodiment does not specifically limit the manner in which the coating slurry is applied to the workpiece surface. For example, the chromizing slurry is applied to the workpiece surface by spraying or brushing.
[0056] It should be noted that the present embodiment does not specifically limit the temperature of drying and curing and sintering treatment. For example, the temperature of drying and curing is 60-300°C and the time is 5min-150min, and the temperature of sintering treatment is 980-1150°C and the time is 8-30min.
[0057] In some preferred embodiments, the drying and curing adopts a segmented gradient curing process, for example, pre-drying at 60-85°C for 5-30 minutes, then drying at 100-160°C for 30-60 minutes, and finally medium-temperature curing at 250-300°C for 20-60 minutes. The segmented curing process ensures that the coating slurry will not have surface quality problems due to local stress during the curing process, and is beneficial to increase the adhesion of the coating.
[0058] In other preferred embodiments, in order to prevent the oxidation of the components in the slurry in the air at high temperature, inert gas protection is used throughout the sintering process, and the workpiece is chromized by rapid heating, and then cooled with the furnace. The sintering temperature is 980℃, 1000℃, 1050℃, 1100℃, 1150℃, and the time is 8min, 15min, 20min, 30min. The thickness of the slurry to be coated under this process is 0.5-1.0mm, and the thickness of the chromium-rich corrosion-resistant coating obtained on the surface of the workpiece after treatment is about 5-50μm.
[0059] S130, spraying or coating a layer of super hydrophobic material on the surface of the chromium-rich corrosion-resistant coating, and obtaining the chromium-rich corrosion-resistant coating through curing. The thickness of the composite coating is 13-64 μm.
[0060] Specifically, a layer of super hydrophobic material is sprayed or coated on the surface of the chromium-rich corrosion-resistant coating, including:
[0061] Anhydrous ethanol, HDTMS and nano-alumina particles are mixed to prepare a suspension, and HDTMS-modified super-hydrophobic Al2O3 nanoparticles are obtained through stirring, centrifugation and drying.
[0062] Epoxy resin, polydimethylsiloxane, epoxy resin curing agent, and Al2O3 nanoparticles treated with HDTMS hydrophobicity are dissolved in xylene to prepare a suspension, which is sprayed on the surface of the chromium-rich corrosion-resistant coating, and a super-hydrophobic / chromium-rich corrosion-resistant composite coating is obtained after curing.
[0063] In some preferred embodiments, the volume of anhydrous ethanol is preferably 45-55 mL, for example, 45 mL, 50 mL, 55 mL, etc., the volume of hexadecyltrimethoxysilane (HDTMS) is preferably 0.5 mL, 1 mL, 1.5 mL, etc., and the content of nano-alumina particles is preferably 1 g, 2 g, 3 g, etc.
[0064] It should be noted that the present embodiment does not specifically limit the mixing method of anhydrous ethanol, HDTMS and nano-alumina particles. For example, each component is placed in a constant temperature magnetic stirrer and stirred for 12 hours to make the alumina particles evenly distributed in the suspension, and super-hydrophobic Al2O3 nanoparticles modified with HDTMS are obtained by centrifugation. Thereafter, the formed nanoparticles are washed with anhydrous ethanol and dried at 120°C for 3 hours to obtain super-hydrophobic Al2O3 nanoparticles modified with HDTMS.
[0065] In other preferred embodiments, the content of epoxy resin (EP) is preferably 0.5-1.5g, for example, 0.5g, 1g, 1.5g, etc., the content of polydimethylsiloxane (PDMS) is preferably 0.5-0.7g, for example, 0.5g, 0.6g, 0.67g, 0.7g, etc., the content of HDTMS hydrophobically treated Al2O3 nanoparticles is preferably 1-2g, for example, 1g, 1.5g, 2g, etc., and the volume of xylene is preferably 10-30mL, for example, 10mL, 15mL, 20mL, 25mL, 30mL, etc.
[0066] In other preferred embodiments, the ratios of EP and PDMS to the curing agent are 3:1 and 10:1 respectively. That is, the ratio of EP to the epoxy resin curing agent is 3:1, and the ratio of PDMS to the curing agent is 10:1.
[0067] It should be further explained that the present embodiment does not specifically limit the treatment method of dissolving epoxy resin, polydimethylsiloxane, epoxy resin curing agent, and Al2O3 nanoparticles treated with HDTMS hydrophobicity in xylene to prepare a suspension. For example, each component is dissolved in xylene, and then the Al2O3 nanoparticles treated with HDTMS hydrophobicity are added, and heated in a constant temperature water bath at 50°C for 1 hour to uniformly disperse them to obtain a suspension.
[0068] In other preferred embodiments, the process parameters for spraying the suspension on the surface of the chromium-rich corrosion-resistant coating are: the spray gun / substrate distance is 15 to 20 cm, for example, 15 cm, 18 cm, 20 cm, and the spray pressure is 0.8 MPa.
[0069] In other preferred embodiments, the curing temperature may be preferably 90-110°C, for example, 90°C, 95°C, 100°C, 110°C, and the curing time may be 1-3h, for example, 1h, 2h, 3h.
[0070] In this embodiment, a hydrophobic film can be formed on the surface of the workpiece through super hydrophobic treatment, so that water vapor cannot stay on the surface of the workpiece, ensuring that the inner surface of the pipeline is dry, thereby improving its comprehensive performance such as corrosion resistance and wear resistance. In addition, this process can also eliminate surface microscopic defects and improve its glossiness and flatness.
[0071] The preparation method of this embodiment is simple and does not need to be carried out under vacuum conditions. At the same time, the chromizing coating has high preparation efficiency, low pollution, adjustable thickness, good wear resistance, and especially excellent resistance to high and low temperature corrosion and steam oxidation. It also has super hydrophobic properties, which can prevent metal oxidation corrosion caused by water vapor, thereby solving the problem of pipeline oxidation corrosion from the root.
[0072] In another aspect of the present disclosure, a hydrophobic / chromium-rich corrosion-resistant composite coating is provided, which is prepared according to the preparation method described above.
[0073] Another aspect of the present disclosure provides an application of a hydrophobic / chromium-rich corrosion-resistant composite coating, wherein the hydrophobic / chromium-rich corrosion-resistant composite coating described above is applied to the inner surface of a boiler pipe.
[0074] The coating of this embodiment has good surface quality, strong surface hydrophobic effect, excellent corrosion resistance and oxidation resistance, and can be applied to various metal parts that need to be strengthened, such as various carbon steels, austenitic steels and high-temperature alloys.
[0075] The preparation method of the hydrophobic / chromium-rich corrosion-resistant composite coating will be further described below in conjunction with several specific examples:
[0076] Example 1
[0077] This example takes a large boiler pipe made of carbon steel as an example to prepare a hydrophobic / chromium-rich corrosion-resistant composite coating. The pipe specifications are all 55mm in outer diameter, 8mm in wall thickness, and 4000mm in length. The steps are as follows:
[0078] S1. Pipeline surface cleaning
[0079] Use alcohol or acetone to remove oil stains, dust, etc. on the surface of the pipe, and use a steel brush to remove the surface oxide.
[0080] S2. Pipeline preheating treatment
[0081] The pipe was preheated at 220°C for 30 min.
[0082] S3. Slurry coating on pipeline surface
[0083] The coating slurry is applied to a suitable thickness at one time by spraying (or by brushing, etc.), and multiple layer coating is not allowed; the coating slurry layer thickness is 0.5mm.
[0084] The preparation method of the coating slurry is as follows: according to the mass percentage of the solid phase components, 60% of chromium powder, 15% of nickel powder, 5% of iron powder, 5% of aluminum powder and 15% of yttrium oxide are weighed respectively, and the mixed metal mixed powder is ball-milled at a ball milling speed of 350r / min and a ball milling time of 8h to obtain the final solid phase component. According to the mass percentage of the liquid phase component, 25% of Al(H2PO4)3, 18% of water glass, 7% of ammonium iodide, 15% of polyvinyl alcohol and 35% of Cr2O3 are measured and mixed to obtain the liquid phase component. The solid phase component and the liquid phase component are mixed at a solid-liquid (g:ml) ratio of 10:2 to obtain the final coating slurry.
[0085] S4, drying and curing
[0086] The metal pipe coated with the chromizing material was pre-dried at 60°C for 5 minutes, then dried at 100°C for 55 minutes, and finally cured at 250°C for 30 minutes.
[0087] S5, fast sintering
[0088] The pipeline is rapidly sintered, diffused and chromized by rapid heating, and then air-cooled to room temperature; the heating rate is set at 1000°C / min, the holding temperature is 980°C, and the holding time is 8min.
[0089] S6. Super hydrophobic treatment
[0090] 50mL of anhydrous ethanol, 1mL of hexadecyltrimethoxysilane (HDTMS) and 2g of nano-alumina particles were made into a suspension, stirred with a constant temperature magnetic stirrer for 12h to make the alumina particles evenly distributed in the suspension, and super-hydrophobic Al2O3 nanoparticles modified by HDTMS were obtained by centrifugation. The formed nanoparticles were washed with anhydrous ethanol and dried at 120℃ for 3h. 1g of epoxy resin (EP) and 0.67g of polydimethylsiloxane (PDMS) were completely dissolved in 20mL of xylene, and the ratios of EP and PDMS curing agent were 3:1 and 10:1, respectively. Then 1.5g of Al2O3 nanoparticles treated with HDTMS hydrophobicity were added, and heated in a constant temperature water bath at 50℃ for 1h to make them evenly dispersed to obtain a suspension. Finally, the suspension was sprayed on the surface of the chromium-rich corrosion-resistant coating, with a spray gun / substrate distance of 15cm and a spray pressure of 0.8MPa. After curing at 100°C for 2h, a composite corrosion-resistant coating was obtained, and the coating thickness was about 13 μm.
[0091] The static water contact angle of the hydrophobic / chromium-rich corrosion-resistant composite coating prepared in Example 1 is 154.1°, and the rolling angle is 2.3°. The water droplets can roll freely on the surface of the coating prepared in Example 1, and after 80 sandpaper wear tests (the coating sample is placed face down on a piece of sandpaper (2000 mesh) under a load of 100g, and moved 20cm along a ruler with the help of a horizontal external force, which is defined as one test cycle), the coating still maintains good superhydrophobic properties.
[0092] Furthermore, the charge transfer resistance (RCT) value of the hydrophobic / chromium-rich corrosion-resistant composite coating prepared in Example 1 in a 3.5 wt. % sodium chloride solution was significantly increased by more than 7 orders of magnitude, and the corrosion inhibition rate reached 99.99%.
[0093] Example 2
[0094] This example takes a large boiler pipe made of austenitic steel as an example to prepare a hydrophobic / chromium-rich corrosion-resistant composite coating. The pipe specifications are all 55mm in outer diameter, 8mm in wall thickness, and 4000mm in length. The steps are as follows:
[0095] S1. Pipeline surface cleaning
[0096] Use alcohol or acetone to remove oil stains, dust, etc. on the surface of the pipe, and use a steel brush to remove the surface oxide.
[0097] S2. Pipeline preheating treatment
[0098] The pipe was preheated at 220°C for 20 min.
[0099] S3. Slurry coating on pipeline surface
[0100] The coating slurry is applied to a suitable thickness at one time by spraying (or by brushing, etc.), and multiple layer coating is not allowed; the coating slurry layer thickness is 0.5mm.
[0101] The preparation method of the coating slurry is as follows: according to the mass percentage of the solid phase components, 70% of chromium powder, 15% of nickel powder, 5% of iron powder, 5% of aluminum powder and 5% of yttrium oxide are weighed respectively, and the mixed metal mixed powder is ball-milled at a ball milling speed of 350r / min and a ball milling time of 10h to obtain the final solid phase component. According to the mass percentage of the liquid phase component, 30% of Al(H2PO4)3, 25% of water glass, 10% of ammonium iodide, 15% of polyvinyl alcohol and 20% of curing agent are measured and mixed to obtain the liquid phase component. The solid phase component and the liquid phase component are mixed at a solid-liquid (g:ml) ratio of 10:3 to obtain the final coating slurry.
[0102] S4, drying and curing
[0103] The metal pipe coated with the chromizing material was pre-dried at 70°C for 5 minutes, then dried at 120°C for 55 minutes, and finally cured at 300°C for 30 minutes.
[0104] S5, fast sintering
[0105] The pipeline is rapidly sintered, diffused and chromized by rapid heating, and then air-cooled to room temperature; the heating rate is set to 1000°C / min, the holding temperature is 1080°C, and the holding time is 20min.
[0106] S6. Super hydrophobic treatment
[0107] A layer of super-hydrophobic material is directly sprayed or coated on the surface of the prepared chromium-rich corrosion-resistant coating. The spraying process is the same as that in Example 1. After curing treatment, a composite corrosion-resistant coating is obtained. The coating thickness is about 43 μm.
[0108] The static water contact angle of the hydrophobic / chromium-rich corrosion-resistant composite coating prepared in Example 2 is 155.6°, and the rolling angle is 1.8°. The water droplets can roll freely on the surface of the coating prepared in Example 2, and after 80 sandpaper wear tests (the coating sample is placed face down on a piece of sandpaper (2000 mesh) under a load of 100g, and moved 20cm along a ruler with the help of a horizontal external force, which is defined as one test cycle), the coating still maintains good superhydrophobic properties.
[0109] Furthermore, the charge transfer resistance (RCT) value of the hydrophobic / chromium-rich corrosion-resistant composite coating prepared in Example 2 in a 3.5 wt. % sodium chloride solution is also increased by more than 7 orders of magnitude, and the corrosion inhibition rate also reaches 99.99%.
[0110] Example 3
[0111] This example takes a large boiler pipe made of high-temperature alloy as an example to prepare a hydrophobic / chromium-rich corrosion-resistant composite coating. The pipe specifications are all 55mm in outer diameter, 8mm in wall thickness, and 4000mm in length, including the following steps:
[0112] S1. Pipeline surface cleaning
[0113] Use alcohol or acetone to remove oil stains, dust, etc. on the surface of the pipe, and use a steel brush to remove the surface oxide.
[0114] S2. Pipeline preheating treatment
[0115] The pipe was preheated at 220°C for 50 min.
[0116] S3. Slurry coating on pipeline surface
[0117] The coating slurry is applied to a suitable thickness at one time by spraying (or by brushing, etc.), and multiple layer coating is not allowed; the coating slurry layer thickness is 1.0mm.
[0118] The preparation method of the coating slurry is as follows: according to the mass percentage of the solid phase components, 70% of chromium powder, 5% of nickel powder, 5% of iron powder, 5% of aluminum powder and 15% of yttrium oxide are weighed respectively, and the mixed metal mixed powder is ball-milled at a ball milling speed of 350r / min and a ball milling time of 12h to obtain the final solid phase component. According to the mass percentage of the liquid phase component, 30% of Al(H2PO4)3, 20% of water glass, 5% of ammonium iodide, 15% of polyvinyl alcohol and 30% of curing agent are measured and mixed to obtain the liquid phase component. The solid phase component and the liquid phase component are mixed at a solid-liquid (g:ml) ratio of 10:5 to obtain the final coating slurry.
[0119] S4, drying and curing
[0120] The metal pipe coated with the chromizing material was pre-dried at 80°C for 10 minutes, then dried at 150°C for 30 minutes, and finally cured at 300°C for 20 minutes.
[0121] S5, fast sintering
[0122] The pipeline is rapidly sintered, diffused and chromized by rapid heating, and then air-cooled to room temperature; the heating rate is set to 1000°C / min, the holding temperature is 1150°C, and the holding time is 30min.
[0123] S6. Super hydrophobic treatment
[0124] A layer of super-hydrophobic material is directly sprayed or coated on the surface of the prepared chromium-rich corrosion-resistant coating. The spraying process is the same as that in Example 1. After curing treatment, a composite corrosion-resistant coating is obtained. The coating thickness is about 64 μm.
[0125] The static water contact angle of the hydrophobic / chromium-rich corrosion-resistant composite coating prepared in Example 3 is 154.5°, and the rolling angle is 2.7°. The water droplets can roll freely on the surface of the coating prepared in Example 3, and after 80 sandpaper wear tests (the coating sample is placed face down on a piece of sandpaper (2000 mesh) under a load of 100g, and moved 20cm along a ruler with the help of a horizontal external force, which is defined as one test cycle), the coating still maintains good superhydrophobic properties.
[0126] Furthermore, the charge transfer resistance (RCT) value of the hydrophobic / chromium-rich corrosion-resistant composite coating prepared in Example 3 in a 3.5 wt. % sodium chloride solution is also increased by more than 7 orders of magnitude, and the corrosion inhibition rate also reaches 99.99%.
[0127] The present disclosure provides a hydrophobic / chromium-rich corrosion-resistant composite coating and a preparation method and application thereof, which have the following beneficial effects compared with the prior art:
[0128] First, the present invention combines chromizing treatment with surface hydrophobic treatment, so that the workpiece surface has not only wear-resistant and corrosion-resistant properties, but also hydrophobic properties, which can prevent metal oxidation corrosion caused by water vapor, thereby solving the problem of pipeline oxidation corrosion from the root;
[0129] Second, the chromizing treatment disclosed in the present invention has high efficiency, low pollution, and adjustable coating thickness.
[0130] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present disclosure, but the present disclosure is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and substance of the present disclosure, and these modifications and improvements are also considered to be within the scope of protection of the present disclosure.
Claims
1. A method for preparing a hydrophobic / chromium-rich corrosion-resistant composite coating, It is characterized in that The preparation method comprises: Preheating the workpiece; The coating slurry is coated on the surface of the workpiece after preheating, and after drying, curing and sintering, a chromium-rich corrosion-resistant coating is obtained on the surface of the workpiece; the coating slurry includes a solid phase component and a liquid phase component; wherein the solid phase component includes chromium powder, nickel powder, iron powder and rare earth compounds; the liquid phase component includes Al(H 2 PO 4 ) 3 , water glass, ammonium halide, polyvinyl alcohol and Cr 2 O 3 ; A layer of super hydrophobic material is sprayed on the surface of the chromium-rich corrosion-resistant coating, and a hydrophobic / chromium-rich corrosion-resistant composite coating is obtained through curing.
2. The preparation method according to claim 1, It is characterized in that The solid-to-liquid ratio of the solid phase component to the liquid phase component is 10:(1-5).
3. The preparation method according to claim 1, It is characterized in that The content of the chromium powder is 40-80%; The content of the nickel powder is 5-30%; The content of the iron powder is 2-20%; The content of the rare earth compound is 5-45%.
4. The preparation method according to claim 1, It is characterized in that The Al(H 2 PO 4 ) 3 The content is 10-30%; The content of water glass is 15-25%; The content of the ammonium halide is 5 to 10%; The content of polyvinyl alcohol is 10-35%; The Cr 2 O 3 The content is 10-30%.
5. The preparation method according to claim 1, It is characterized in that The rare earth compound is a rare earth oxide or a rare earth chloride; and / or, The ammonium halide is ammonium bromide or ammonium iodide.
6. The preparation method according to any one of claims 1 to 5, It is characterized in that A layer of super hydrophobic material is sprayed on the surface of the chromium-rich corrosion-resistant coating, and a hydrophobic / chromium-rich corrosion-resistant composite coating is obtained through curing, comprising: Anhydrous ethanol, HDTMS and nano-alumina particles were mixed to prepare a suspension, and super-hydrophobic Al2O3 modified with HDTMS was obtained by stirring, centrifuging and drying. 2 O 3 Nanoparticles; Epoxy resin, polydimethylsiloxane, epoxy resin curing agent, HDTMS hydrophobic treated Al 2 O 3 The nanoparticles are dissolved in xylene to prepare a suspension, which is sprayed on the surface of the chromium-rich corrosion-resistant coating to obtain a super-hydrophobic / chromium-rich corrosion-resistant composite coating after curing.
7. The preparation method according to any one of claims 1 to 5, It is characterized in that The workpiece preheating treatment temperature is 150-220°C and the time is 30-60 minutes; and / or, Under the protection of inert gas, the sintering temperature is 980-1150°C and the time is 8-30 minutes.
8. The preparation method according to any one of claims 1 to 5, It is characterized in that The thickness of the chromium-rich corrosion-resistant coating is 5 to 50 μm; and / or, The thickness of the hydrophobic / chromium-rich corrosion-resistant composite coating is 13-64 μm.
9. A hydrophobic / chromium-rich corrosion-resistant composite coating, It is characterized in that Prepared according to the preparation method according to any one of claims 1 to 8.
10. Application of a hydrophobic / chromium-rich corrosion-resistant composite coating, It is characterized in that The hydrophobic / chromium-rich corrosion-resistant composite coating according to claim 9 is applied to the inner surface of the boiler pipe.
Citation Information
Cited By
Preparation method of slurry-method chromium-nickel co-permeation coating of liquid-phase multi-component binder
CN119824364A