Two-component alkaline silver removal agent and silver removal process thereof

Through the combination of two-component alkaline desilverizer and sustained-release reducing capsules, the oxidation and reduction of silver is accelerated by using alkaline metal salts and sustained-release reducing agents, and combined with lead powder to modify the ceratops, the danger of acidic desilverizer is solved. The problem of efficiency and inefficiency has achieved efficient and environmentally friendly silver recycling.

CN118932336APending Publication Date: 2024-11-12JIANGMEN UBIS SEMICON MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411016366.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-27
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing acidic silver desilver agents are highly dangerous and prone to corrode the underlying alloy, making it difficult to directly dissolve the silver layer, resulting in a low silver desilver rate and is not environmentally friendly.

Method used

Using a two-component alkaline desilverizer, the oxidation of silver is accelerated by the alkaline metal salt solution in component A, combined with the sustained-release reducing capsule in component B, the reducing agent is released under strong alkali, and complex is formed to carry out silver. Recycle and accelerate the oxidation reaction through lead powder modified ceramic granules to avoid corrosion of the underlying metal.

Benefits of technology

It realizes rapid and safe and efficient recycling of silver ingots, avoids environmental pollution, improves silver removal rate and rate, and ensures the safety of the lower alloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004965813410000051
    Figure BDA0004965813410000051
  • Figure BDA0004965813410000061
    Figure BDA0004965813410000061
  • Figure BDA0004965813410000071
    Figure BDA0004965813410000071
Patent Text Reader

Abstract

The invention relates to the technical field of silver removal and recovery, and particularly discloses a bi-component alkaline silver removal agent and a silver removal process thereof. The bi-component alkaline silver removal agent comprises a component A and a component B, the component A is prepared from the following raw materials in parts by weight: 100 to 160 parts of strong alkali solution and 23 to 66 parts of alkali metal salt; the component B is prepared from the following raw materials in parts by weight: 90 to 150 parts of NH3.H2O, 60 to 100 parts of slow-release reduction capsules and 20 to 40 parts of water. The silver removal process comprises the following steps: S1, soaking the component A to prepare silver oxide; s2, adding a component B to remove silver oxide; and S3, silver recovery, wherein the silver complex solution is filtered, washed, dried and cast to obtain 99.6% silver ingots. The alkaline silver removal agent prepared in the invention can be used for quickly soaking and removing silver on complex parts which are difficult to physically remove silver, and has the advantages of high silver removal rate, recoverability and high silver removal speed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of desilvering and recovery technology, and more specifically, to a two-component alkaline desilvering agent and a desilvering process thereof. Background Art With the development of electronic devices and semiconductor manufacturing industries, and in order to improve the performance of electronic devices, a variety of surface processing methods for devices have been studied, among which silver plating technology is more common. The silver-plated layer can improve the thermal conductivity and electrical conductivity of the device, enhance the welding performance, and is easy to polish and has strong reflective ability, thereby improving the aesthetics of the device. At present, metallic silver is widely used, which also derives the problem of how to simply and efficiently deal with waste silver-plated devices. Acidic desilvering agents are highly dangerous and easily corrode the alkali metals or alloys under the silver layer and cannot be widely used, and silver is difficult to dissolve directly in alkaline solutions. Therefore, it is necessary to develop an alkaline desilvering agent and desilvering process that can simply and quickly dissolve the silver layer, does not damage the underlying alloy, and has a high desilvering rate. Summary of the invention

[0003] In order to prepare a desilvering agent with a faster desilvering process and a higher desilvering rate, the present application provides a two-component alkaline desilvering agent and a desilvering process thereof.

[0004] In the first aspect, the present application provides a two-component alkaline desilvering agent, which adopts the following technical solution: A two-component alkaline desilvering agent comprises a component A and a component B. The raw materials of the component A comprise, by weight, 100-160 parts of a strong alkaline solution and 23-66 parts of an alkali metal salt; the raw materials of the component B comprise, by weight, 90-150 parts of NH3·H2O, 60-100 parts of a sustained-release reduction capsule and 20-40 parts of water.

[0005] By adopting the above technical scheme, the alkaline metal salt solution in component A and the silver-containing workpiece can form a primary battery to accelerate the oxidation reaction of silver, and oxidize the metallic silver into silver oxide in a short time; after adding component B, the shell of the sustained-release reduction capsule encounters a strong alkali and dissolves, releasing the internal reducing agent to reduce the silver oxide, at which time the reduced silver ions and ammonium ions combine in the solution to form a complex and leave; although the acidic desilvering agent also has a good silver removal effect, it will react with the underlying alkali metal, and the desilvering agent of the present application is an alkaline system, so there will be no problem of corrosion of the underlying metal, and the silver ingot can be recovered after filtering, washing, drying, melting and casting.

[0006] Preferably, the raw materials of the sustained-release reduced capsule in component B are: 10-30 parts by weight of glucose, 20-40 parts by weight of formaldehyde, 50-70 parts by weight of water, 5-15 parts by weight of microcrystalline cellulose, and 60-120 parts by weight of polyethylene terephthalate.

[0007] Preferably, the preparation method of the sustained-release reduction capsule in the B component is: firstly, glucose, water, formaldehyde and microcrystalline cellulose are mixed and stirred until uniform, then granulated, and finally polyethylene terephthalate is coated on the outer layer by spray drying to form a microcapsule shell.

[0008] By adopting the above technical scheme, microcrystalline cellulose can make the morphology of the internal reducing component more stable, which is beneficial to controlling the uniformity of the granulation size and has a high application rate after being made into microcapsules. Using polyethylene terephthalate as the outer shell of the reducing microcapsule can exist for a long time in a weak alkaline environment, and when encountering a strong alkali, it dissolves and releases the internal glucose and formaldehyde as reducing agents to participate in the reaction. The stability of the reaction can be controlled through the sustained release effect, and the reducing substances in the alkali solution can be replenished in time to assist the large-scale and rapid complexation of silver ions, thereby optimizing the silver removal effect.

[0009] Preferably, the strong alkaline solution is any one or more of sodium hydroxide and potassium hydroxide aqueous solutions; the alkali metal salt is any one or two of sodium nitrate and potassium nitrate.

[0010] Preferably, the raw material of component A further comprises 1-3 parts by weight of metal lead powder modified ceramsite, wherein the modified ceramsite is prepared by bonding porous ceramsite and nano metal lead powder with epoxy resin adhesive.

[0011] By adopting the above technical scheme, the speed of the oxidation reaction of silver in the formed primary battery can be increased by adding lead powder. The porous structure of the ceramsite modified by lead powder can be used to load more lead powder on its surface. Since the ceramsite and lead powder have better integrity after bonding, the lead powder-modified ceramsite is more convenient to remove and reuse, and it will not cause lead-containing wastewater to avoid environmental pollution.

[0012] In a second aspect, the present application provides a desilvering process using a two-component alkaline desilvering agent, which adopts the following technical solution: A desilvering process using a two-component alkaline desilvering agent, comprising the following steps: S1. Immerse half of the workpiece to be treated with silver on the surface in component A and place the other half in the air. Heat the liquid of component A to 50-60°C and stir continuously. After reacting for 2-4 hours, turn the workpiece in the opposite direction and continue to immerse for 2-4 hours to obtain a silver oxide workpiece. S2, continue to immerse the silver oxide workpiece in the original alkaline component A and cool it to room temperature, and directly add the component B, stir evenly and make the silver oxide workpiece to be treated completely immersed in the desilvering agent, soak for 3-6 hours, obtain the desilvered workpiece and take it out, and the solution after immersion is a silver complex solution; S3. Recovering silver: filtering, washing, drying, and melting the silver complex solution to obtain silver ingots.

[0013] Preferably, the silver-containing workpiece to be processed is also subjected to a pre-oxidation operation of soaking in hydrogen peroxide for 1-3 minutes.

[0014] Preferably, when filtering the silver complex in step S3, the waste liquid obtained after filtering out the silver complex is heated and concentrated and can be reused as component A.

[0015] In summary, this application has the following beneficial effects: 1. In the present application, the alkaline metal salt solution in component A and the silver-containing workpiece can form a primary battery to accelerate the oxidation reaction of silver, and oxidize the metallic silver into silver oxide in a short time; after the addition of component B, the shell of the sustained-release reduction capsule dissolves when encountering a strong alkali, and the reducing agent inside is released to reduce the silver oxide. At this time, the reduced silver ions and ammonium ions combine in the solution to form a complex and leave, and the silver ingot can be recovered after filtration, washing, drying, melting and casting.

[0016] 2. In the present application, the lead powder-modified ceramsite can improve the speed of the oxidation reaction of silver in the formed primary battery, and will not cause lead-containing wastewater to avoid environmental pollution. A weak alkali-resistant material is used as the outer shell of the reduction microcapsule. Only when it is mixed with component A and encounters a strong alkali, it dissolves and releases the internal reducing agent to overflow and participate in the reaction. The slow release effect during the dissolution process can control the stability of the reduction reaction and provide timely replenishment of the reducing substances that are constantly consumed in the alkali solution, thereby assisting the large-scale and rapid complexation of silver ions, improving the silver removal rate and silver removal rate, and optimizing the silver removal effect. DETAILED DESCRIPTION

[0017] The present application is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the experiments are carried out according to conventional conditions or the conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources.

[0018] The preparation method of the metal lead powder modified ceramsite in the present application is to bond 10kg of porous ceramsite and 10kg of nano-grade metal lead powder with 5kg of epoxy resin, and the specific operation is to mix the ceramsite and lead powder and then add the epoxy resin and stir to obtain the ceramsite; wherein the epoxy resin is produced by Shanghai Shouxing ME300 epoxy resin adhesive, the particle size of porous ceramsite is 8mm, and the particle size of nano metal lead powder is 5nm.

[0019] Preparation Example of Sustained Release Reduction Capsules Preparation Example 1 The preparation method of the sustained-release reduced capsule in component B is as follows: first, 10 kg of glucose, 20 kg of formaldehyde, 50 kg of water, and 5 kg of microcrystalline cellulose are mixed and stirred at a speed of 600 rpm for 15 minutes until uniform, and then transferred to a granulator for granulation to form microparticles with a particle size of less than 20 nm, and finally the microparticles are coated by spray drying, the spray pressure is set to 1.0 MPa, 60 kg of polyethylene terephthalate is sprayed and coated on the outer layer of the microparticles, and then solidified to form a microcapsule shell.

[0020] Preparation Example 2 The preparation method of the sustained-release reduction capsule in component B is as follows: first, 20 kg of glucose, 30 kg of formaldehyde, 60 kg of water, and 10 kg of microcrystalline cellulose are stirred at a rotation speed of 600 rpm for 15 minutes until they are uniform, and then transferred to a granulator for granulation to form microparticles with a particle size of less than 20 nm, and finally the microparticles are coated by a spray drying method, the spray pressure is set to 1.0 MPa, 90 kg of polyethylene terephthalate is sprayed and coated on the outer layer of the microparticles, and then solidified to form a microcapsule shell.

[0021] Preparation Example 3 The preparation method of the sustained-release reduced capsule in component B is as follows: first, 30 kg of glucose, 40 kg of formaldehyde, 70 kg of water, and 15 kg of microcrystalline cellulose are stirred at a rotation speed of 600 rpm for 15 minutes until they are uniform, and then transferred to a granulator for granulation to form microparticles with a particle size of less than 20 nm, and finally the microparticles are coated by a spray drying method, the spray pressure is set to 1.0 MPa, 120 kg of polyethylene terephthalate is sprayed and coated on the outer layer of the microparticles, and then solidified to form a microcapsule shell.

[0022] Preparation Example 4 The preparation method of the sustained-release reduced capsule in component B is as follows: first, 10 kg of glucose, 20 kg of formaldehyde, 50 kg of water, and 5 kg of microcrystalline cellulose are mixed and stirred at a speed of 600 rpm for 15 minutes until uniform, and then transferred to a granulator for granulation to form microparticles with a particle size of less than 20 nm. Finally, the microparticles are coated by spray drying, and the spray pressure is set to 1.0 MPa. 60 kg of polyethylene glycol-6000 ester is sprayed out and coated on the outer layer of the microparticles, and then solidified to form a microcapsule shell.

[0023] Preparation Example 5 The preparation method of the sustained-release reduced capsule in component B is as follows: 50 kg of water and 5 kg of microcrystalline cellulose are mixed and stirred at a speed of 600 rpm for 15 minutes until uniform, and then transferred to a granulator for granulation to form microparticles with a particle size of less than 20 nm. Finally, the microparticles are coated by spray drying, and the spray pressure is set to 1.0 MPa. 60 kg of polyethylene terephthalate is sprayed and coated on the outer layer of the microparticles, and then solidified to form a microcapsule shell. Example

[0024] Example 1 A desilvering process using a two-component alkaline desilvering agent comprises the following steps: S1. Soak 50% of the volume of the workpiece to be treated with silver on the surface in component A, and expose 50% of the volume to the air. Heat the liquid of component A to 50°C and stir it continuously. After reacting for 2 hours, turn the workpiece in the opposite direction and continue soaking for 4 hours to obtain a silver oxide workpiece. S2, continue to immerse the silver oxide workpiece in the original alkaline component A and cool it to room temperature, and directly add the component B, stir evenly and make the silver oxide workpiece to be treated completely immersed in the desilvering agent, soak for 6 hours, obtain the desilvered workpiece and take it out, and the remaining components are the silver complex solution; S3. Recovering silver: filtering, washing, drying the silver complex solution, and then melting and casting to obtain silver ingots.

[0025] Example 2 A desilvering process using a two-component alkaline desilvering agent comprises the following steps: S1, immerse half of the workpiece to be treated with silver on the surface in component A, and place the other half in the air, heat the liquid of component A to 55°C, and stir continuously, react for 3 hours, turn the workpiece to the opposite direction and continue to immerse for 3 hours, so as to obtain a silver oxide workpiece; S2, continue to immerse the silver oxide workpiece in the original alkaline component A, cool to room temperature, and directly add component B, stir evenly and make the silver oxide workpiece to be treated completely immersed in the desilvering agent, soak for 3-6 hours, obtain the desilvered workpiece and take it out, and the remaining components are silver complex solution; S3. Recovering silver: filtering, washing, drying the silver complex solution, and then melting and casting to obtain silver ingots.

[0026] Example 3 A desilvering process using a two-component alkaline desilvering agent comprises the following steps: S1, immerse half of the workpiece to be treated with silver on the surface in component A, and place the other half in the air, heat the liquid of component A to 60°C, and stir continuously, react for 4 hours, turn the workpiece to the opposite direction and continue to immerse for 2 hours, and obtain a silver oxide workpiece; S2, continue to immerse the silver oxide workpiece in the original alkaline component A, cool to room temperature, and directly add component B, stir evenly and make the silver oxide workpiece to be treated completely immersed in the desilvering agent, soak for 3 hours, obtain the desilvered workpiece and take it out, and the remaining components are silver complex solution; S3. Recovering silver: filtering, washing, drying the silver complex solution, and then melting and casting to obtain silver ingots.

[0027] The amounts of raw materials added in Examples 1-9 are detailed in the table below; Example 10 The method of Example 1 is followed, except that the concentrated recovery liquid is reused as component A, that is, component A is replaced in equal amounts with the concentrated recovery liquid having a pH value of 13.8.

[0028] According to the process steps in Example 1, the similarities and differences of the desilvering processes of Examples 4-10 are shown in the table below; <![CDATA[Whether to perform H2O2 pre-oxidation]]> Volume of liquid immersed in component A Example 4 no 50% volume Example 5 no 50% volume Example 6 no 50% volume Example 7 no 50% volume Example 8 no Immerse yourself in everything Example 9 Yes, pre-oxidation for 2 minutes 50% volume Example 10 no 50% volume Comparative Example Comparative Examples 1-4 were carried out according to the method of Example 1, and the differences in the amounts of raw materials added are shown in the following table; Performance testing 1. Silver layer oxidation rate detection 2. Silver removal rate detection Detection Methods 1. Silver layer oxidation rate detection: prepare several 1kg iron-carbon alloy test blocks plated with 10g silver coating, and then operate according to the desilvering process in the embodiment and the comparative example; calculate the silver layer oxidation rate by weighing the mass after the formation of silver oxide, and record the silver layer oxidation rate results of each embodiment and comparative example after soaking for 20min, 40min, 1h, 2h, and 3h, respectively. The faster the speed of silver oxide generation in the silver layer, the faster the desilvering speed of the subsequent addition of component B is. Therefore, the desilvering speed of the desilvering agent can be reflected by comparing the change rate of the oxidation rate. The silver layer oxidation rate detection results of each embodiment are shown in Table 1, and the silver layer oxidation rate detection results of the comparative example are shown in Table 2; 2. Silver removal rate detection: A 1 kg iron-carbon alloy test block originally plated with 10 g silver coating that had been immersed in component A was immersed in component B. The silver removal rate was calculated by weighing the mass of the alloy block after immersion for 1 h, 2 h, and 3 h. The test results of each embodiment are shown in Table 3, and the test results of the comparative example are shown in Table 4.

[0029] Table 1 Table 2 Test items Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 20min 31% 30% 5% 5% 40min 55% 52% 14% 9% 1h 73% 71% 19% 11% 2h 80% 79% 22% 12% 3h 86% 84% 23% 12% Table 3 Table 4 Combining the performance test results of Example 1 and Example 4, it can be seen that due to the replacement of the microcapsule shell material, the effect of being soluble in a strong alkaline solution and insoluble under weak alkaline conditions cannot be achieved, and the reducing substance therein overflows in large quantities when not mixed with component A, losing the sustained release effect, and the reducing substance is easy to react with oxygen in the air and lose its activity, resulting in a slowdown in the desilvering speed and a decrease in the desilvering rate.

[0030] It can be seen from the performance test results of Example 1 and Example 5 that replacing alkaline substances other than sodium hydroxide and potassium hydroxide will cause the desilvering effect to deteriorate due to problems such as reduced alkalinity strength, and the desilvering rate and desilvering rate will decrease.

[0031] Combining the performance test results of Example 1 and Example 6, it can be seen that after the lead powder is used to modify the ceramsite, the oxidation rate of the silver layer in the original battery is significantly improved due to the catalytic effect of the lead powder, thereby accelerating the silver removal speed and achieving a better silver removal effect; Combining the performance test results of Example 1 and Example 7, it can be seen that the catalytic effect is not much different from that of adding modified ceramsite, but the lead powder overflows and cannot be collected for reuse, and the waste liquid formed contains a large amount of heavy metal lead powder, which will cause water pollution.

[0032] Combining the performance test results of Example 1 and Example 8, it can be seen that when the silver-plated alloy block is completely immersed in component A, the silver-plated alloy block cannot form a primary cell with the salt solution in the desilvering agent, and therefore cannot accelerate the oxidation of the silver layer, resulting in a decrease in oxidation efficiency and slower silver oxide generation, and the desilvering rate of the complexed silver oxide within a subsequent limited time is also reduced.

[0033] Combining the performance test results of Example 1 and Example 9, it can be seen that the initial generation rate of silver oxide has increased, and the oxidation rate in the early stage has obviously accelerated, so the time cost of the desilvering process has been reduced and the economic benefit has been improved.

[0034] Combining the test results of Example 1 and Example 10, it can be seen that the alkali solution can be reused multiple times through the recovery and concentration operation, and the difference in the desilvering effect is not large, which saves the raw material cost of the desilvering agent and avoids material waste.

[0035] It can be seen from the performance test results of Example 1 and Comparative Example 1 that without a sustained-release capsule shell, the effect of being soluble in a strong alkaline solution and insoluble under a weak alkaline condition cannot be achieved, and the reducing substance is easy to react with oxygen in the air and loses its activity when not mixed with component A, resulting in a slowdown in the desilvering speed and a reduction in the desilvering rate.

[0036] Combining the performance test results of Example 1 and Comparative Example 2, it can be seen that when no metal salt is added, the silver-plated alloy block cannot form a primary cell with the salt solution in the desilvering agent, and therefore cannot accelerate the oxidation of the silver layer, resulting in a decrease in oxidation efficiency and slower silver oxide generation, and the desilvering rate of the complexed silver oxide within a subsequent limited time is also reduced.

[0037] It can be seen from the performance test results of Example 1 and Comparative Example 3 that only immersion in component B can remove a small part of the silver coating, but the desilvering effect in the embodiment cannot be achieved at all, and the requirement of removing most of the silver is not met.

[0038] It can be seen from the performance test results of Example 1 and Comparative Example 4 that no obvious desilvering effect can be achieved without adding a reducing agent.

[0039] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A two-component alkaline desilvering agent, characterized in that: The invention comprises component A and component B. The raw materials of component A comprise, by weight, 100-160 parts of strong alkaline solution and 23-66 parts of alkali metal salt; the raw materials of component B comprise, by weight, 90-150 parts of NH3·H2O, 60-100 parts of sustained-release reduction capsules and 20-40 parts of water.

2. A two-component alkaline desilvering agent according to claim 1, characterized in that The raw materials of the sustained-release reduced capsule in component B are: 10-30 parts by weight of glucose, 20-40 parts by weight of formaldehyde, 50-70 parts by weight of water, 5-15 parts by weight of microcrystalline cellulose, and 60-120 parts by weight of polyethylene terephthalate.

3. A two-component alkaline desilvering agent according to claim 2, characterized in that: The preparation method of the sustained-release reduction capsule in the B component is: firstly, glucose, water, formaldehyde and microcrystalline cellulose are mixed and stirred until uniform, then granulated, and finally polyethylene terephthalate is coated on the outer layer by spray drying to form a microcapsule shell.

4. A two-component alkaline desilvering agent according to claim 1, characterized in that: The strong alkaline solution is selected from any one or more of sodium hydroxide and potassium hydroxide aqueous solutions; the alkali metal salt is selected from any one or two of sodium nitrate and potassium nitrate.

5. A two-component alkaline desilvering agent according to claim 1, characterized in that: The raw material of component A also includes 1-3 parts by weight of metal lead powder modified ceramsite, and the modified ceramsite is prepared by bonding porous ceramsite and nano metal lead powder with epoxy resin adhesive.

6. A desilvering process, characterized in that: The method is realized by a two-component alkaline desilvering agent as claimed in claim 1, comprising the following steps: S1. Immerse half of the workpiece to be treated with silver on the surface in component A and place the other half in the air. Heat the liquid of component A to 50-60°C and stir continuously. After reacting for 2-4 hours, turn the workpiece in the opposite direction and continue to immerse for 2-4 hours to obtain a silver oxide workpiece. S2, continue to immerse the silver oxide workpiece in the original alkaline component A and cool it to room temperature, and directly add the component B, stir evenly and make the silver oxide workpiece to be treated completely immersed in the desilvering agent, soak for 3-6 hours, obtain the desilvered workpiece and take it out, and the solution after immersion is a silver complex solution; S3. Recovering silver: filtering, washing, drying, and melting the silver complex solution to obtain silver ingots.

7. The desilvering process of a two-component alkaline desilvering agent according to claim 6, characterized in that: The silver-containing workpiece to be processed is also subjected to a pre-oxidation operation of being immersed in hydrogen peroxide for 1-3 minutes.

8. A two-component alkaline desilvering agent according to claim 3, characterized in that: When filtering the silver complex in step S3, the waste liquid obtained after filtering out the silver complex can be heated and concentrated and reused as component A.