Compound corrosion inhibitor for pipeline steel as well as preparation method and application of compound corrosion inhibitor
By combining the corrosion inhibitor of sodium tungstate, L-phenylalanine and zinc gluconate, combined with the adsorption layer and precipitation film-type corrosion inhibition, the problem of low corrosion inhibition efficiency of sodium tungstate alone is solved, and high efficiency is achieved Pipe steel has anti-corrosion effect and reduces production costs.
Patent Information
- Application Number
- CN202411003600.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
AI Technical Summary
When existing corrosion inhibitors use sodium tungstate in industrial applications, their corrosion inhibition efficiency is low when used alone, which cannot meet industrial needs. Some harmful corrosion inhibitors are prohibited. It is necessary to develop environmentally friendly compounding solutions to improve corrosion inhibition efficiency. .
Using a composite corrosion inhibitor of sodium tungstate, L-phenylalanine and zinc gluconate, an adsorption layer is formed on the metal surface by sodium tungstate and L-phenylalanine, and a precipitated film-type corrosion inhibitor of zinc gluconate It can be used to form a synergistic effect to improve corrosion inhibition performance and is suitable for anti-corrosion of pipeline steel in acidic environments such as petroleum.
The corrosion inhibition efficiency has been significantly improved, from about 60% to 85-90%, and the production cost has been reduced, achieving efficient corrosion resistance to pipeline steel. At the same time, the material is non-toxic and stable and easy to store and mass production.
Smart Images

Figure CN118932338A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a compound corrosion inhibitor, in particular to a compound corrosion inhibitor for pipeline steel, and also to a preparation method and application of the corrosion inhibitor. Background Art
[0002] Corrosion inhibitor is a chemical substance or a mixture of several chemical substances that can prevent or slow down corrosion when it exists in the environment (medium) in an appropriate concentration and form. Generally speaking, corrosion inhibitors refer to substances that are used to protect metal surfaces. Adding trace or small amounts of such chemicals can significantly reduce the corrosion rate of metal materials in the medium to zero. At the same time, the original physical and mechanical properties of the metal material can be kept unchanged. Reasonable use of corrosion inhibitors is an effective way to prevent corrosion of metals and their alloys in environmental media. Corrosion inhibitor technology has become one of the most widely used methods in anti-corrosion technology due to its good effects and high economic benefits. Especially in the production and processing of petroleum products, chemical cleaning, atmospheric environment, industrial water, machinery, instrument manufacturing and petrochemical production processes, corrosion inhibition technology has become one of the main anti-corrosion means.
[0003] Most of the existing corrosion inhibitors are anodic or cathodic corrosion inhibitors, because some harmful polluting environments have been banned by the state. Adsorption film type is relatively less used, and usually needs to be compounded with other corrosion inhibitors to achieve the expected effect, and the cost is relatively high. Sodium tungstate, as a non-toxic and harmless inorganic corrosion inhibitor, is expected to be promoted and applied in environmentally friendly corrosion inhibitors. However, the use of sodium tungstate alone not only requires a large amount of use, but also has a low corrosion inhibition rate, which cannot meet industrial requirements. Therefore, it is necessary to strengthen the research on the compounding scheme of sodium tungstate corrosion inhibitors to improve the corrosion inhibition efficiency of such corrosion inhibitors. Summary of the invention
[0004] Purpose of the invention: The purpose of the present invention is to provide a composite corrosion inhibitor for pipeline steel, and also to provide a method for preparing the above-mentioned corrosion inhibitor and its application in the corrosion protection of pipeline steel in an acidic environment such as one rich in petroleum.
[0005] Technical solution: The composite corrosion inhibitor for pipeline steel of the present invention comprises the following raw materials per liter: 100-800 mg sodium tungstate, 0.005-0.1 mol L-phenylalanine, 2-20 mg zinc gluconate, and the rest is water.
[0006] Wherein, the pH value of the corrosion inhibitor is 7-8.
[0007] Wherein, the corrosion inhibitor is of analytical grade.
[0008] The preparation method of the above-mentioned composite corrosion inhibitor comprises the following steps:
[0009] (1) Take 15-60% of the volume of water to prepare the target corrosion inhibitor;
[0010] (2) Sodium tungstate, L-phenylalanine and zinc gluconate are taken and dissolved in water to obtain sodium tungstate corrosion inhibition solution, L-phenylalanine corrosion inhibition solution and zinc gluconate corrosion inhibition solution;
[0011] (3) The sodium tungstate corrosion inhibitor, L-phenylalanine corrosion inhibitor and zinc gluconate corrosion inhibitor are mixed and stirred until completely mixed, and then the remaining water is added to make up the volume and stirred evenly to obtain a composite corrosion inhibitor for oil pipelines.
[0012] Wherein, in step (2), the amount of water used is 50-200 ml; the volume of sodium tungstate corrosion inhibitor, L-phenylalanine corrosion inhibitor and zinc gluconate corrosion inhibitor is 50-200 ml, and the volume ratio is 1:1:1.
[0013] The above-mentioned composite corrosion inhibitor for pipeline steel can be used for corrosion protection of pipeline steel in acidic environments such as those rich in petroleum.
[0014] The ratio of the concentration of the corrosive liquid in the pipeline steel to the concentration of the corrosion inhibitor is 1:1.5 to 2, preferably 1:2.
[0015] Specifically, the application is to configure a composite corrosion inhibitor for pipeline steel according to the concentration of corrosive liquid in the oil pipeline, use a pipeline corrosion inhibitor plug, and cover the composite corrosion inhibitor for pipeline steel on the inner surface of the pipeline under the push of gas, and then pass the corrosive liquid after drying.
[0016] Furthermore, during the application process, the corrosiveness of the corrosion liquid after corrosion inhibition is monitored using on-site exploration instruments, and the protective effect of the corrosion inhibitor is determined. After the corrosion inhibition effect decreases, repeated coating can be performed to restore or increase the corrosion inhibition effect.
[0017] Invention principle: The corrosion inhibitor of the present invention is to combine sodium tungstate with Zn+ and L-phenylalanine to produce adsorption on the metal surface, thereby hindering the corrosion process of the metal surface to achieve the effect of corrosion inhibition. Among them, L-phenylalanine is the basic component of protein, and its molecule contains amino and carboxyl groups with corrosion inhibition effect, and it is non-toxic to the environment and can be completely decomposed in the natural environment.
[0018] The corrosion inhibition mechanism of L-phenylalanine is that L-phenylalanine contains non-polar benzene ring, polar group -NH2 and carboxyl group. The lone pair of electrons contained in the central atom N of the polar group -NH2 coordinates with the empty d electron orbit of iron and can be adsorbed on the surface of iron to form a film; the hydrophilic carboxyl group carries more negative charges and can provide electrons to the empty orbit of iron, thereby forming a stable and dense chemical adsorption protective film on the surface of steel; the hydrophobic benzene ring forms a directional arrangement upward, and as a result, the corrosive medium is arranged and squeezed out by the corrosion inhibitor molecules, so that the medium is separated from the metal surface, which plays a role in protecting the metal. Sodium tungstate, as a corrosion inhibitor for uniform corrosion of metals in solution, changes the active polarization of metals and inhibits pitting corrosion of metals. According to the passive film theory, tungstates can fill gaps and repair defects in metal oxide films. Oxide films are mainly iron oxides formed in the air, which have defects and pores. Tungstate ions react with iron ions in the solution to form iron tungstate or ferrous tungstate, which cover the metal surface together with the oxidation products, filling pores and repairing defects, reducing the activation points of corrosion. Zinc salt corrosion inhibitor is a typical precipitation film type corrosion inhibitor. Its mechanism of action is mainly to form a Zn(OH)2 precipitation film in the local alkaline environment of the cathode, preventing oxygen from diffusing to the metal surface, thereby playing a protective role. Therefore, the presence of sodium tungstate in zinc salt can reduce tungstate ions to low-valent tungsten oxide, which can improve the corrosion resistance of steel. At the same time, the role of the carboxyl group in L-phenylalanine can promote the formation of Zn(OH)2 precipitation film. There is a synergistic effect of corrosion inhibition among the three, which greatly improves the corrosion resistance of metals. It is also very suitable for anti-corrosion treatment of pipeline steel in acidic environments such as those rich in petroleum, inhibiting the formation of the main corrosion products Fe2O3 and FeS in the pipeline, and promoting the formation of other product films such as tungsten oxide and zinc hydroxide oxide film on the inner surface of the pipeline, thereby improving the corrosion resistance of steel.
[0019] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) Sodium tungstate can achieve a synergistic corrosion inhibition effect after being compounded with zinc gluconate and L-phenylalanine, which can effectively improve the corrosion inhibition performance. Compared with the single sodium tungstate corrosion inhibitor, after adding zinc gluconate and L-phenylalanine, the corrosion inhibition efficiency is increased from about 60% to 85-90%; (2) The corrosion inhibitor of the present invention has a simple use process, good corrosion inhibition effect, low production cost, stable corrosion inhibitor, easy storage and mass production, and has extremely high practical application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is the polarization curve of X65MS pipeline steel in the composite corrosion inhibitor of the present invention;
[0021] Figure 2 Polarization curves of X65MS pipeline steel in different concentrations of sodium tungstate corrosion inhibitor;
[0022] Figure 3Polarization curves of X65MS pipeline steel in different concentrations of L-phenylalanine corrosion inhibitor;
[0023] Figure 4 Polarization curves of X65MS pipeline steel in different concentrations of zinc gluconate corrosion inhibitor. DETAILED DESCRIPTION
[0024] The technical scheme of the present invention is further described below in conjunction with the examples. The test materials used in the examples can all be purchased through conventional channels.
[0025] Example 1
[0026] The composite corrosion inhibitor for pipeline steel of the present invention comprises the following raw materials: sodium tungstate, L-phenylalanine, zinc gluconate and water.
[0027] (1) Take 15% of the volume of water to prepare the target corrosion inhibitor;
[0028] (2) Weigh analytical grade sodium tungstate and add water to prepare 50 ml of 100, 200, 300, 400, 500, and 800 mg / L sodium tungstate corrosion inhibition solutions respectively;
[0029] Weigh analytically pure L-phenylalanine, add water, and prepare 50 ml of 0.005, 0.01, 0.05, and 0.1 mol / L L-phenylalanine corrosion inhibition solutions, respectively;
[0030] Weigh analytically pure zinc gluconate, add water, and prepare 50 ml of 2, 8, and 20 mg / L zinc gluconate corrosion inhibition solutions, respectively;
[0031] (3) The three corrosion inhibition solutions were taken, mixed thoroughly and then fixed to 1 L. Sodium tungstate, L-phenylalanine and zinc gluconate were compounded to study their synergistic effect, and the corrosion inhibition effect of the composite corrosion inhibitor for pipeline steel of the present invention was verified.
[0032] Based on the corrosion inhibition performance of X65MS pipeline steel using three corrosion inhibitors, sodium tungstate, L-phenylalanine and zinc gluconate, the appropriate concentration range was determined by the relationship between the corrosion inhibition efficiency and concentration of a single corrosion inhibitor. An orthogonal experiment was conducted using L9 (34) with concentration as the level and the type of corrosion inhibitor as the factor. The orthogonal experiment is shown in Table 1:
[0033] Table 1. L9 (34) factor level table of the composite corrosion inhibitor for pipeline steel of the present invention
[0034]
[0035]
[0036] The corrosion inhibition efficiency is calculated by using the polarization curves of the samples corresponding to each experimental number in the orthogonal experimental table shown in Table 1 and is shown in Table 2.
[0037] Table 2. Analysis of orthogonal test results of the composite corrosion inhibitor for pipeline steel of the present invention
[0038]
[0039] From Table 2, we can see that the order of influence of the three factors ABC is C>B>A, that is, zinc gluconate is the main influencing factor, L-phenylalanine is second, and sodium tungstate has a smaller influence. The blank range (0.049) is smaller than the zinc gluconate range (0.071), but larger than the sodium tungstate range (0.036) and L-phenylalanine range (0.042), indicating that there is non-negligible interaction between the experimental factors. This shows that the orthogonal experiment is feasible.
[0040] The average values indicate that the best concentration ratio of the ternary compound is 300 mg / L sodium tungstate, 0.1 mol / L L-phenylalanine, and 20 mg / L zinc gluconate, that is, the A2B2C3 combination is the best.
[0041] Based on the best combination obtained from the orthogonal experiment, parallel verification results are as follows Figure 1 As shown. The corrosion inhibition efficiency of the ternary compound corrosion inhibitor with a ratio of 300 mg / L sodium tungstate, 20 mg / L zinc gluconate and 0.1 mol / L L-phenylalanine for X65MS pipeline steel in H2S medium can reach about 91%. The corrosion inhibition efficiency of the compound of sodium tungstate, zinc gluconate and L-phenylalanine is significantly better than that of a single corrosion inhibitor. This is because the N atom on the guanidine group of the L-phenylalanine side chain and the N atom on the amino group-NH2 both contain lone pairs of electrons. The lone pairs of electrons are coordinated and combined with the empty orbits on the metal iron, so that the metal iron atoms form a more stable electron layer arrangement structure, so that arginine is adsorbed on the surface of the metal iron to form a dense oxide film, which prevents the contact between the corrosive medium and the metal surface and protects the metal matrix. At the same time, zinc gluconate, as a strong reducing agent, passivates the metal surface, and tungstic acid is reduced with ions to generate low-priced tungsten oxide, which can improve the corrosion resistance of steel. Therefore, there is a good synergistic effect between sodium tungstate, zinc gluconate and L-phenylalanine. In addition, sodium tungstate, zinc gluconate and L-phenylalanine are non-toxic and harmless substances, and L-phenylalanine can be biodegraded in the natural environment. Zinc gluconate is relatively cheap, thereby reducing the cost of the composite corrosion inhibitor.
[0042] Comparative Example 1
[0043] The steel corrosion inhibitor of Comparative Example 1 has the following components and contents: 100, 200, 300, 400, 500, 800 mg / L of sodium tungstate, and the rest is water.
[0044] The preparation method of the above corrosion inhibitor, taking the preparation of 100 ml of corrosion inhibitor as an example, specifically comprises the following steps:
[0045] (1) Take 4 beakers of the same size and add 50 ml of 3.5 wt% NaCl + 0.005 mol / L Na2S2O3 solution;
[0046] (2) Add 50 ml of the prepared 100, 200, 300, 400, 500, and 800 mg / L sodium tungstate solution to the solution obtained in step (1), stir evenly until completely dissolved to obtain a mixed solution, and measure the pH with a Cantonese pH test paper to verify that the pH value of the obtained solution is about 7, which is close to neutral.
[0047] The method for using the above steel corrosion inhibitor is that the electrode material is X65MS steel, and the X65MS pipeline steel is processed into a sample with an outer size of 10mm×10mm×5mm by a machine. The wire is welded to the back of the working surface of the sample with tin liquid, and the sample is placed therein and sealed with epoxy resin; then, the working surface of the X65MS pipeline steel is polished step by step with 400#-2000# sandpaper until the surface is smooth. The polished sample is cleaned with anhydrous ethanol and deionized water, degreased with acetone, and dried with cold air for use.
[0048] The three-electrode system was used for measurement. The research electrode was X65MS pipeline steel, the reference electrode was a silver chloride electrode, and the auxiliary electrode was a platinum electrode. The research electrodes were immersed in different concentrations of sodium tungstate corrosion inhibitors, and a three-electrode system was formed with a saturated silver chloride electrode and a platinum electrode for electrochemical testing. The scanning speed was 0.5mV / s during the steady-state polarization curve measurement, and the scanning range was -300 to 300mV relative to the open circuit potential. The electrode potentials were all relative to the silver chloride electrode potential.
[0049] like Figure 2 As shown in the figure, it is the polarization curve of X65MS pipeline steel in different concentrations of sodium tungstate corrosion inhibitor. It can be seen from the figure that when no corrosion inhibitor is added, the anodic overpotential and cathodic overpotential of the corrosion polarization curve of X65MS pipeline steel in the corrosive solution are not much different, so its corrosion should be a mixed control process. It can also be seen from the figure that the addition of sodium tungstate has an inhibitory effect on the corrosion of X65MS pipeline steel. As the concentration of sodium tungstate increases, the inhibitory effect on the anodic process increases. When the concentration reaches 300mg / L, the inhibitory effect weakens. The fitting data of the polarization curve are shown in Table 3:
[0050] Table 3. Polarization curve fitting parameters of X65MS pipeline steel in different concentrations of sodium tungstate corrosion inhibitor
[0051]
[0052] As the concentration of sodium tungstate increases, the self-corrosion current decreases. When the concentration is 300 mg / L, the self-corrosion current is the smallest. Then, as the concentration continues to increase, the self-corrosion current also increases. After adding the corrosion inhibitor, the self-corrosion potential of X65MS pipeline steel is greater than that without adding the corrosion inhibitor, that is, the self-corrosion potential shifts positively after adding the corrosion inhibitor, which shows that the inhibitor of sodium tungstate has a significantly greater inhibitory effect on the anodic reaction of the corrosion process than on the cathodic reaction. Therefore, it can be considered that this corrosion inhibitor is an anodic corrosion inhibitor, and its reaction mechanism may be to passivate the metal to form a passivation film to inhibit corrosion.
[0053] Comparative Example 2
[0054] The steel corrosion inhibitor of Comparative Example 2 has the following components and contents: 0.005, 0.01, 0.05, 0.1 mol / L of L-phenylalanine, and the rest is water.
[0055] The preparation method of the above corrosion inhibitor, taking the preparation of 100 ml of corrosion inhibitor as an example, specifically comprises the following steps:
[0056] (1) Take 4 beakers of the same size and add 50 ml of 3.5 wt% NaCl + 0.005 mol / L Na2S2O3 solution;
[0057] (2) Add 50 ml of the prepared 0.005, 0.01, 0.05, and 0.1 mol / L L-phenylalanine solutions to the solution obtained in step (1), respectively, stir evenly until completely dissolved to obtain a mixed solution, and measure the pH with a Cantonese pH test paper to verify that the pH value of the obtained solution is about 7, which is close to neutral.
[0058] The method for using the above-mentioned corrosion inhibitor is that the electrode material is X65MS steel, and the X65MS pipeline steel is processed into a sample with an outer size of 10mm×10mm×5mm by a machine. The wire is welded to the back of the working surface of the sample with tin liquid, and the sample is placed therein and sealed with epoxy resin; then, the working surface of the X65MS pipeline steel is polished step by step with 400#-2000# sandpaper until the surface is smooth. The polished sample is cleaned with anhydrous ethanol and deionized water, degreased with acetone, and dried with cold air for use.
[0059] The three-electrode system was used for measurement. The research electrode was X65MS pipeline steel, the reference electrode was a silver chloride electrode, and the auxiliary electrode was a platinum electrode. The research electrodes were immersed in different concentrations of L-phenylalanine corrosion inhibitor, and a three-electrode system was formed with a saturated silver chloride electrode and a platinum electrode for electrochemical testing. The scanning speed was 0.5mV / s during the steady-state polarization curve measurement, and the scanning range was -300 to 300mV relative to the open circuit potential. The electrode potentials were all relative to the silver chloride electrode potential.
[0060] like Figure 3The polarization curves of X65MS pipeline steel in different concentrations of L-phenylalanine corrosion inhibitor are shown in Table 4. The fitting parameters obtained by Tafel fitting are shown in Table 4:
[0061] Table 4. Polarization curve fitting parameters of X65MS pipeline steel in different concentrations of L-phenylalanine inhibitor
[0062]
[0063] Compared with the blank solution, the corrosion potential of X65MS pipeline steel in the solution containing LPHA has a certain degree of positive shift, but the positive shift is very small, less than 50mV, and the corrosion potential changes very little with the increase of LPHA concentration. At the same time, after adding LPHA, the cathode and anode polarization current densities of the X65MS pipeline steel electrode both decrease, indicating that the addition of LPHA can simultaneously inhibit the anodic reaction and cathodic reaction of X65MS pipeline steel. Therefore, LPHA is a mixed inhibitor for X65MS pipeline steel in the corrosion solution, and its mechanism of action is the geometric coverage effect. It can also be seen from Table 2 that with the increase of X65MS pipeline steel concentration after LPHA, the corrosion current density of the X65MS pipeline steel electrode decreases and the corrosion inhibition efficiency increases. After adding LPHA, the inhibitory effect of the electrode reaction of X65MS pipeline steel is enhanced.
[0064] Comparative Example 3
[0065] The steel corrosion inhibitor of Comparative Example 3 has the following components and contents: 2, 8, and 20 mg / L zinc gluconate, and the rest is water.
[0066] The preparation method of the above steel corrosion inhibitor, taking the preparation of 100 ml of corrosion inhibitor as an example, specifically comprises the following steps:
[0067] (1) Take 4 beakers of the same size and add 50 ml of 3.5 wt% NaCl + 0.005 mol / L Na2S2O3 solution;
[0068] (2) Add 50 ml of the prepared 2, 8, and 20 mg / L zinc gluconate solutions to the solution obtained in step (1), respectively, stir evenly until completely dissolved to obtain a mixed solution, and measure the pH with a Cantonese pH test paper to verify that the pH value of the obtained solution is about 7, which is close to neutral.
[0069] The method for using the above steel corrosion inhibitor is that the electrode material is X65MS steel, and the X65MS pipeline steel is processed into a sample with an outer size of 10mm×10mm×5mm by a machine. The wire is welded to the back of the working surface of the sample with tin liquid, and the sample is placed therein and sealed with epoxy resin; then, the working surface of the X65MS pipeline steel is polished step by step with 400#-2000# sandpaper until the surface is smooth. The polished sample is cleaned with anhydrous ethanol and deionized water, degreased with acetone, and dried with cold air for use.
[0070] The three-electrode system was used for measurement. The research electrode was X65MS pipeline steel, the reference electrode was a silver chloride electrode, and the auxiliary electrode was a platinum electrode. The research electrodes were immersed in zinc gluconate corrosion inhibitors of different concentrations, and a three-electrode system was formed with a saturated silver chloride electrode and a platinum electrode for electrochemical testing. The scanning speed was 0.5mV / s during the steady-state polarization curve measurement, and the scanning range was -300 to 300mV relative to the open circuit potential. The electrode potentials were all relative to the silver chloride electrode potential.
[0071] like Figure 4 The polarization curves of X65MS pipeline steel in different concentrations of zinc gluconate corrosion inhibitor are shown in Table 5.
[0072] Table 5. Polarization curve fitting parameters of X65MS pipeline steel in different concentrations of zinc gluconate inhibitor
[0073]
[0074] It can be seen from the data in the table that after adding ZnGL concentration to 20 mg / L, the corrosion current is 3.948 μA / cm2 lower than that of the blank test. 2 Reduced to 1.592μA / cm 2 , and with the increase of agent concentration, the corrosion current decreases more significantly. At the same time, it can be seen from the significant decrease in βc value that ZnGL mainly controls the cathode hydrogen evolution reaction. This is because Zn 2+ A Zn(OH)2 precipitation film is formed in the local alkaline environment of the cathode to prevent carbon steel from contacting with corrosive ions. According to the changes in βa and Ecorr, ZnGL is a mixed corrosion inhibitor that mainly controls the cathode. It may be that the adsorption of gluconate restricts the diffusion of the anode area to interfere with the anode process. When the ZnGL concentration is 20 mg / L, the corrosion inhibition rate reaches the highest 59.69%.
[0075] contrast Figures 1 to 4According to the experimental data, when sodium tungstate, zinc gluconate and L-phenylalanine exist alone, the corrosion inhibition efficiency of steel reaches 60.03%, 59.69% and 61.79%. When the three corrosion inhibitors are compounded according to the optimal ratio and concentration, the corrosion inhibition efficiency of the ternary compound corrosion inhibitor for X65MS pipeline steel in H2S medium can reach about 91%, which is about 30% higher than that of the single corrosion inhibition rate, which is a significant improvement for oil pipeline corrosion inhibition. The corrosion inhibition efficiency of sodium tungstate, zinc gluconate and L-phenylalanine after compounding is significantly better than that of a single corrosion inhibitor because L-phenylalanine contains non-polar benzene rings, polar groups -NH2 and carboxyl groups. The lone pair of electrons contained in the central atom N of the polar group -NH2 coordinates with the empty d electron orbit of iron and can be adsorbed on the iron surface to form a film. At the same time, zinc gluconate, as a strong reducing agent, passivates the metal surface, and tungstic acid is reduced with ions to generate low-valent tungsten oxide, which can improve the corrosion resistance of steel. Therefore, sodium tungstate, zinc gluconate and L-phenylalanine have a good synergistic effect and achieve a strong corrosion inhibition effect. In addition, due to the non-toxic and harmless effect of the corrosion inhibitor, it is a green corrosion inhibitor for oil pipelines with development potential.
Claims
1. A composite corrosion inhibitor for pipeline steel, It is characterized in that The corrosion inhibitor comprises the following raw materials per liter: 100-800 mg of sodium tungstate, 0.005-0.1 mol of L-phenylalanine, 2-20 mg of zinc gluconate, and the rest is water.
2. The composite corrosion inhibitor according to claim 1, It is characterized in that The pH value of the corrosion inhibitor is 7-8.
3. The composite corrosion inhibitor according to claim 1, It is characterized in that The corrosion inhibitor is of analytical grade.
4. A method for preparing the composite corrosion inhibitor according to claim 1, It is characterized in that The following steps are involved: (1) Take 15-60% of the volume of water to prepare the target corrosion inhibitor; (2) Sodium tungstate, L-phenylalanine and zinc gluconate are taken and dissolved in water to obtain sodium tungstate corrosion inhibition solution, L-phenylalanine corrosion inhibition solution and zinc gluconate corrosion inhibition solution; (3) The sodium tungstate corrosion inhibitor, L-phenylalanine corrosion inhibitor and zinc gluconate corrosion inhibitor are mixed and stirred until completely mixed, and then the remaining water is added to make up the volume and stirred evenly to obtain a composite corrosion inhibitor for oil pipelines.
5. The method according to claim 4, It is characterized in that In step (2), the amount of water used is 50 to 200 ml.
6. Use of the composite corrosion inhibitor for pipeline steel according to claim 1 for corrosion protection of pipeline steel in an acidic environment rich in petroleum.
7. The use according to claim 6, It is characterized in that The ratio of the concentration of corrosive liquid in pipeline steel to the concentration of corrosion inhibitor is 1:1.5~2.
8. The use according to claim 6, It is characterized in that The application is specifically to configure a composite corrosion inhibitor for pipeline steel according to the concentration of corrosive liquid in the oil pipeline, and to use a pipeline corrosion inhibitor plug to cover the composite corrosion inhibitor for pipeline steel on the inner surface of the pipeline under the push of gas.