Method for cleaning aviation aluminum alloy sheet parts before spot welding
By adopting the environmentally friendly cleaning methods of manual cleaning, degreasing, alkaline washing, pickling and drying processes before spot welding of aviation aluminum alloy thin plate parts, the problems of long process time, serious environmental pollution and low production efficiency in the prior art are solved. It achieves efficient and environmentally friendly pre-spot welding cleaning effect, is suitable for automated production and reduces costs.
Patent Information
- Application Number
- CN202410994992.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-24
AI Technical Summary
The existing pre-spot welding cleaning process of aerospace aluminum alloy thin plate parts has problems such as long process time, low production efficiency, serious environmental pollution and high cost. It is especially difficult to adapt to large-scale production and automated production, and Cr6+ is often used. Pickling methods cannot meet environmental protection needs.
Using a pre-spot welding cleaning method including manual cleaning, degreasing, alkali washing, pickling and drying, using environmentally friendly solutions such as Isoprep44, a mixed solution of NaOH and NaCO3, a mixed solution of Bonderite C-IC2310 Aero and nitric acid, etc., through Multiple washes and deionized water washes remove surface contaminants, the process time is shortened to a minimum of 2.5 minutes, and does not contain Cr6+, suitable for collinear production and automated production.
It significantly improves production efficiency, reduces process time and cost, reduces environmental pollution, achieves environmental protection effects, and is suitable for multi-model, multi-process collinear production without the need to build new or remodel production lines.
Smart Images

Figure CN118932342A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to aluminum alloy surface treatment technology, and in particular to a method for cleaning aviation aluminum alloy thin plate parts before spot welding. Background Art
[0002] In aviation manufacturing, aluminum alloy sheets are widely used in aircraft fuselages, wings, bulkheads and other structures due to their good strength and toughness, easy processing and corrosion resistance. As the main method for fixing and connecting thin plate parts, spot welding has high welding quality, small deformation, high energy efficiency and fast welding speed, and can provide a strong connection without adding too much weight. The main factor affecting the quality of spot welding is contact resistance, so all spot welds need to be cleaned before spot welding to remove the surface oxide film or contaminants, thereby reducing the contact resistance. At present, there are many ways to clean before spot welding, and the commonly used method is multiple pickling. For example, the spot welding cleaning process currently used by Xi'an Aircraft Industry Corporation includes two mixed acid treatment processes, namely nitric chromium pickling and phosphorus chromium pickling. If the process contains an alkaline washing process, an additional nitric chromium pickling is required, and the main process time (alkaline washing + pickling) is nearly 30 minutes. Although multiple pickling has a good effect, it will lead to a long process time, excessive part thinning, and the risk of dimensional deviation. In addition, it will seriously affect production efficiency in mass production, especially for automated production lines, which require short pulsation cycles. Multiple pickling methods will seriously affect production cycles and are difficult to adapt to automated production. In addition, in aviation production, since multiple models and multiple processes are involved in co-production, the pickling solution before spot welding of aluminum alloy thin plate parts is often not compatible with the pickling solution before anodizing, and separate tanks or lines need to be built, increasing construction and maintenance costs. In addition, the current pickling method before aluminum alloy spot welding often involves Cr 6+ , which seriously pollutes the environment and greatly increases the cost of wastewater treatment. For example, the patent application number 201310145488.2, "A method for cleaning aluminum alloy aircraft skin before spot welding", uses two pickling processes: chromium sulfuric acid pickling and tri-acid mixed acid pickling, and both contain Cr 6+ , cannot meet the growing environmental protection needs. Summary of the invention
[0003] The purpose of the present invention is to provide a Cr-free and efficient Cr-free ... 6+ A cleaning method for aviation aluminum alloy thin plate parts before spot welding is developed to improve production efficiency, reduce costs and promote environmental protection.
[0004] The object of the present invention is achieved by the following manner: A method for cleaning aviation aluminum alloy thin plate parts before spot welding, which can be used for surface cleaning of 0.5mm-2mm thin plate parts before spot welding, and the process flow includes manual cleaning process, degreasing process, alkali cleaning process, pickling process, drying process and water washing treatment between each process, characterized in that it includes the following steps:
[0005] 1. Manual cleaning process: Wipe the surface of aluminum alloy sheet parts with white cotton cloth dipped in organic solvent to remove residual glue, oil and other pollutants on the surface;
[0006] 2. Degreasing process: Soak the parts in the degreasing solution for 1-20 minutes. The degreasing solution is an aqueous solution of Isoprep44. The concentration of Isoprep44 is 45g / L-75g / L. The temperature of the degreasing solution is 55-65℃. Compressed air is used for stirring during the soaking period. The purpose of degreasing is to further remove residual grease pollutants.
[0007] 3. Warm water washing process: put the degreased parts into warm water and rinse for 1-5 minutes at a water temperature of 30-60°C to remove the degreasing solution remaining on the surface of the parts;
[0008] 4 Cold water washing process: put the parts washed with warm water into cold water for 1-5 minutes, the water temperature is 10-30℃ to further remove the residual degreasing solution;
[0009] 5 Alkali washing process: Soak the parts in the alkaline washing solution for 0.5-3min. The alkaline washing solution is a mixed solution of NaOH and NaCO3. The concentration of NaOH is 20g / L-35g / L, the concentration of NaCO3 is 20g / L-30g / L, and the temperature of the alkaline washing solution is 40-55℃. Compressed air is used for stirring during the alkaline washing process. The purpose of alkaline washing is to remove the oxide scale and pollutants on the surface of the parts;
[0010] 6. Warm water washing process: put the parts after alkali washing into warm water and rinse for 1-5 minutes at a water temperature of 30-60℃ to remove the residual alkali washing solution on the surface of the parts;
[0011] 7 Cold water washing process: put the parts washed with warm water into cold water for 1-5 minutes, the water temperature is 10-30℃ to further remove the residual alkaline washing solution;
[0012] 8 Pickling process: Soak the parts in the pickling solution for 2-15 minutes. The pickling solution is a mixed solution of Bonderite C-IC2310Aero and nitric acid, with a volume fraction of Bonderite C-IC2310 Aero of 10-20%, a volume fraction of nitric acid of 20-30%, and the rest is deionized water. The pickling solution temperature is 10-35°C. When the copper content reaches 0.2g / L or when necessary, 2% volume of Bonderite C-AD Deoxlm 2315Aero can be added to prevent copper redeposition. The purpose of pickling is to further remove the oxide scale on the one hand, and to play a role in lightening after alkaline washing on the other hand;
[0013] 9 Cold water washing process: put the pickled parts into cold water and rinse for 1-5 minutes at a water temperature of 10-30℃ to remove the pickling solution remaining on the surface of the parts;
[0014] 10. Deionized water washing process: wash the parts in deionized water for 1-5 minutes at a water temperature of 10-30°C to further remove the residual pickling solution;
[0015] 11 Drying process: Dry the parts in an oven at 50-70℃ for at least 30 minutes.
[0016] The aluminum alloy parts described in the present invention refer to aluminum alloy thin plate parts made of 2A12, LF2, LF21, LF6 and the like, but are not limited to aluminum alloys of this series and form.
[0017] The organic solvent in step 1 of the present invention includes ethanol, acetone, butanone, ethyl acetate and common commercial cleaning agents.
[0018] The cold water washing in step 4 and the deionized water washing in step 10 of the present invention should be carried out on the basis of achieving a continuous water film state before proceeding to the next step.
[0019] In the water washing process of the present invention, the parts should not be stationary during the process, and the parts should be continuously moved for washing to ensure thorough washing.
[0020] The step 10 of the present invention is to clean with deionized water, including rinsing and spraying.
[0021] The beneficial effects achieved by the present invention are:
[0022] 1. The process time required for cleaning aluminum alloy thin plate parts before spot welding is greatly reduced. The main process (including alkali cleaning and acid cleaning) only takes 2.5 minutes at the shortest. This parameter can meet the cleaning requirements of most aluminum alloy thin plate parts, significantly improve production efficiency, and is more suitable for automated production.
[0023] 2. The process solution used can also be used as a treatment solution in other surface treatment processes such as anodizing, and can be used for co-production without the need to build or renovate production lines, which is convenient to implement.
[0024] 3. The process solutions used do not contain Cr 6+ , reduce environmental pollution, have good environmental protection effects, and reduce wastewater treatment costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a process flow chart of an implementation method of the present application. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical scheme and advantages of the implementation of the present application clearer, the technical scheme in the embodiment of the present application will be described in more detail below in combination with the results in the embodiment of the present application. The described embodiment is a part of the embodiment of the present application, rather than all of the embodiments. The embodiment described below is exemplary and is intended to be used to explain the present application, and cannot be understood as a limitation to the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0027] Embodiment 1:
[0028] Select 2A12 aluminum-clad aluminum alloy test pieces with a thickness of 1.5 mm and test piece numbers 1-1, 1-2, and 1-3, and clean them according to the following steps:
[0029] 1. Manual cleaning process: Wipe the surface of aluminum alloy sheet parts with white cotton cloth dipped in butanone to remove surface contaminants such as residual glue and oil.
[0030] 2. Degreasing process: Soak the aluminum alloy specimen in an aqueous solution of Isoprep44 for 15 minutes. The concentration of Isoprep44 is 50.9 g / L and the solution temperature is 57°C. Compressed air is used for stirring during the soaking period.
[0031] 3. Warm water washing process: Put the degreased aluminum alloy specimen into warm water and rinse for 2 minutes at a water temperature of 47°C.
[0032] 4. Cold water washing process: Put the aluminum alloy specimen after warm water washing into cold water and rinse for 1 minute at a water temperature of 25°C.
[0033] 5. Alkali washing process: Soak the aluminum alloy specimen in a mixed solution of NaOH and NaCO3 for 1 min. The NaOH concentration is 25.1 g / L, the NaCO3 concentration is 24.9 g / L, and the solution temperature is 50°C. Compressed air is used for stirring during the alkaline washing process.
[0034] 6. Warm water washing process: put the aluminum alloy test piece after alkali washing into warm water and rinse for 2 minutes at a water temperature of 47°C.
[0035] 7. Cold water washing process: Put the aluminum alloy specimen after warm water washing into cold water and rinse for 1 minute at a water temperature of 20°C.
[0036] 8. Pickling process: The aluminum alloy specimen was immersed in a mixed solution of Bonderite C-IC2310 Aero and nitric acid for 6 minutes, with the volume fraction of Bonderite C-IC2310 Aero being 12.6%, the volume fraction of nitric acid being 28.3%, and the solution temperature being 20°C.
[0037] 9. Cold water washing process: Rinse the pickled aluminum alloy specimen in cold water for 1 minute at a water temperature of 20°C.
[0038] 10. Deionized water washing process: Rinse the aluminum alloy specimen in deionized water for 2 minutes at a water temperature of 20°C.
[0039] 11. Drying process: Dry the parts in an oven at 55°C for 30 minutes.
[0040] The contact resistance value, surface roughness and thinning amount are shown in the following table:
[0041]
[0042] The results show that this method can obtain qualified contact resistance and surface roughness, and the thinning amount is much less than 50% of the aluminum coating. (The single aluminum coating accounts for at least 4% of the total thickness, about 0.06mm)
[0043] Embodiment 2:
[0044] Select 2A12 aluminum-clad aluminum alloy test pieces, test piece thickness 2.0 mm, test piece number 2-1, 2-2, 2-3, and clean them according to the following steps:
[0045] 1. Manual cleaning process: Wipe the surface of aluminum alloy sheet parts with white cotton cloth dipped in butanone to remove surface contaminants such as residual glue and oil.
[0046] 2. Degreasing process: Soak the aluminum alloy specimen in an aqueous solution of Isoprep44 for 10 minutes. The concentration of Isoprep44 is 52.3 g / L and the solution temperature is 60°C. Use compressed air for stirring during the soaking period.
[0047] 3. Warm water washing process: Put the degreased aluminum alloy specimen into warm water and rinse for 2 minutes at a water temperature of 50°C.
[0048] 4. Cold water washing process: Put the aluminum alloy specimen after warm water washing into cold water and rinse for 1 minute at a water temperature of 20°C.
[0049] 5. Alkali washing process: Soak the aluminum alloy specimen in a mixed solution of NaOH and NaCO3 for 0.5 min. The NaOH concentration is 26.7 g / L, the NaCO3 concentration is 26.9 g / L, the solution temperature is 50°C, and compressed air is used for stirring during the alkaline washing process.
[0050] 6. Warm water washing process: put the aluminum alloy test piece after alkali washing into warm water and rinse for 2 minutes at a water temperature of 50°C.
[0051] 7. Cold water washing process: Put the aluminum alloy specimen after warm water washing into cold water and rinse for 1 minute at a water temperature of 20°C.
[0052] 8. Pickling process: The aluminum alloy specimen was immersed in a mixed solution of Bonderite C-IC2310 Aero and nitric acid for 2 minutes, with the volume fraction of Bonderite C-IC2310 Aero being 12.6%, the volume fraction of nitric acid being 28.3%, and the solution temperature being 20°C.
[0053] 9. Cold water washing process: Rinse the pickled aluminum alloy specimen in cold water for 1 minute at a water temperature of 20°C.
[0054] 10. Deionized water washing process: Rinse the aluminum alloy specimen in deionized water for 2 minutes at a water temperature of 20°C.
[0055] 11. Drying process: Dry the parts in an oven at 55°C for 30 minutes.
[0056] The contact resistance value, surface roughness and thinning amount are shown in the following table:
[0057]
[0058] The results show that this method can obtain qualified contact resistance and surface roughness, and the thinning amount is much less than 50% of the aluminum coating. (The single aluminum coating accounts for at least 4% of the total thickness, about 0.08mm)
[0059] Embodiment 3:
[0060] Select LF6 aluminum alloy test pieces with a thickness of 1.5 mm and test piece numbers 3-1, 3-2, and 3-3, and clean them according to the following steps:
[0061] 1. Manual cleaning process: Wipe the surface of aluminum alloy sheet parts with white cotton cloth dipped in acetone to remove residual glue, oil and other pollutants on the surface.
[0062] 2. Degreasing process: Soak the aluminum alloy specimen in an aqueous solution of Isoprep44 for 10 minutes. The concentration of Isoprep44 is 50.9 g / L and the solution temperature is 57°C. Compressed air is used for stirring during the soaking period.
[0063] 3. Warm water washing process: Put the degreased aluminum alloy specimen into warm water and rinse for 2 minutes at a water temperature of 47°C.
[0064] 4. Cold water washing process: Put the aluminum alloy specimen after warm water washing into cold water and rinse for 1 minute at a water temperature of 20°C.
[0065] 5. Alkali washing process: Soak the aluminum alloy specimen in a mixed solution of NaOH and NaCO3 for 0.5 min, with a NaOH concentration of 25.1 g / L, a NaCO3 concentration of 24.9 g / L, and a solution temperature of 50°C. Compressed air is used for stirring during the alkaline washing process.
[0066] 6. Warm water washing process: put the aluminum alloy test piece after alkali washing into warm water and rinse for 2 minutes at a water temperature of 47°C.
[0067] 7. Cold water washing process: Put the aluminum alloy specimen after warm water washing into cold water and rinse for 1 minute at a water temperature of 20°C.
[0068] 8. Pickling process: The aluminum alloy specimen was immersed in a mixed solution of Bonderite C-IC2310 Aero and nitric acid for 10 minutes, the volume fraction of Bonderite C-IC2310 Aero was 12.4%, the volume fraction of nitric acid was 28.6%, and the solution temperature was 20°C.
[0069] 9. Cold water washing process: Rinse the pickled aluminum alloy specimen in cold water for 1 minute at a water temperature of 20°C.
[0070] 10. Deionized water washing process: Rinse the aluminum alloy specimen in deionized water for 2 minutes at a water temperature of 20°C.
[0071] 11. Drying process: Dry the parts in an oven at 55°C for 30 minutes.
[0072] The contact resistance value, surface roughness and thinning amount are shown in the following table:
[0073]
[0074] The results show that this method can obtain qualified contact resistance and surface roughness, and the thinning amount is also within the allowable range.
Claims
1. A method for cleaning aviation aluminum alloy thin plate parts before spot welding, which can be used for surface cleaning of 0.5mm-2mm thin plate parts before spot welding. The process flow includes manual cleaning process, degreasing process, alkali cleaning process, pickling process, drying process and water washing treatment between each process, characterized in that: The following steps are involved: 1.1 Manual cleaning process: Wipe the surface of aluminum alloy sheet parts with white cotton cloth dipped in organic solvent to remove residual glue and oil contaminants on the surface; 1.2 Degreasing process: Soak the parts in the degreasing solution for 1-20 minutes, and use compressed air to stir during the soaking period to further remove residual grease pollutants; 1.3 Warm water washing process: put the degreased parts into warm water and rinse for 1-5 minutes at a water temperature of 30-60℃ to remove the degreasing solution remaining on the surface of the parts; 1.4 Cold water washing process: put the parts washed with warm water into cold water for 1-5 minutes, the water temperature is 10-30℃ to further remove the residual degreasing solution; 1.5 Alkali washing process: Soak the parts in the alkaline washing solution for 0.5-3 minutes. Use compressed air to stir during the alkaline washing process to remove the oxide scale and pollutants on the surface of the parts; 1.6 Warm water washing process: put the parts after alkali washing into warm water and rinse for 1-5 minutes at a water temperature of 30-60℃ to remove the residual alkali washing solution on the surface of the parts; 1.7 Cold water washing process: put the parts washed with warm water into cold water for 1-5 minutes, the water temperature is 10-30℃, to further remove the residual alkaline washing solution; 1.8 Pickling process: Soak the parts in the pickling solution for 2-15 minutes. Use compressed air to stir during the pickling process. The purpose is to further remove the oxide scale and play a role in shining after alkaline washing. 1.9 Cold water washing process: put the pickled parts into cold water for 1-5 minutes, the water temperature is 10-30℃ to remove the pickling solution remaining on the surface of the parts; 1.10 Deionized water washing process: Wash the parts in deionized water for 1-5 minutes at a water temperature of 10-30°C to further remove the residual pickling solution; 1.11 Drying process: Dry the parts in an oven at 50-70℃ for at least 30 minutes.
2. The method for cleaning aviation aluminum alloy sheet parts before spot welding according to claim 1, characterized in that The degreasing solution is an aqueous solution of Isoprep44, the concentration of Isoprep44 is 45g / L-75g / L, and the temperature of the degreasing solution is 55-65°C.
3. The method for cleaning aviation aluminum alloy sheet parts before spot welding according to claim 1, characterized in that The alkaline washing solution is a mixed solution of NaOH and NaCO3, the NaOH concentration is 20g / L-35g / L, the NaCO3 concentration is 20g / L-30g / L, and the alkaline washing solution temperature is 40-55°C.
4. The method for cleaning aviation aluminum alloy sheet parts before spot welding according to claim 1, characterized in that The pickling solution is a mixed solution of Bonderite C-IC2310 Aero and nitric acid, with a volume fraction of Bonderite C-IC2310 Aero of 10-20%, a volume fraction of nitric acid of 20-30%, and the rest being deionized water; the pickling solution temperature is 10-35°C; when the copper content in the pickling solution reaches 0.2g / L or when necessary, 2% volume of Bonderite C-AD Deoxlm 2315Aero can be added to prevent copper redeposition.
Citation Information
Patent Citations
Aluminum alloy airplane skin cleaning method before spot welding
CN103212550A
Cleaning process / method for aluminum alloy material
CN103806008A
Chemical cleaning method of rust-proof aluminum alloy
CN104213132A
Methods of preparing 7xxx aluminum alloys for adhesive bonding, and products relating to the same