Copper nanowire loaded palladium monatomic composite material as well as preparation method and application thereof

In the electrocatalytic hydrogenation reaction, the palladium single atom composite material is supported by copper nanowires, and the activated hydrogen is provided by using palladium single atom cracking water, which solves the problems of low efficiency and by-product generation in the selective hydrogenation reaction of nitroaromatics, and realizes the problem of low efficiency and by-product generation in the selective hydrogenation reaction of nitroaromatics. Efficient and stable catalytic effect.

CN118932372APending Publication Date: 2024-11-12UNIV OF SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410981333.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the selective hydrogenation catalyst of nitroaromatic hydrocarbons in electrocatalytic hydrogenation reaction is low in efficiency, and there are no related reports on copper-based catalysts in electrocatalytic hydrogenation reactions, so it is difficult to avoid the generation of by-products and maintain other reducing groups. group.

Method used

The copper nanowire-supported palladium single-atom composite material is used as a catalyst to adsorb nitroaromatic hydrocarbons through the copper nanowire support and use palladium single-atom to crack water to provide active hydrogen, which promotes the conversion of nitro groups to amine groups and improves the conversion rate and selectivity of the reaction.

Benefits of technology

High catalytic efficiency, selectivity and stability in the electrochemical hydrogenation reaction of nitroaromatics is achieved, ensuring the generation of target products and avoiding the generation of by-products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004956889890000141
    Figure BDA0004956889890000141
  • Figure HDA0004956889940000011
    Figure HDA0004956889940000011
  • Figure HDA0004956889940000012
    Figure HDA0004956889940000012
Patent Text Reader

Abstract

The invention provides a copper nanowire loaded palladium monatomic composite material as well as a preparation method and application thereof. The copper nanowire loaded palladium single atom composite material comprises a copper nanowire carrier and palladium single atoms loaded on the copper nanowire carrier. Wherein palladium atoms in the copper nanowire loaded palladium monatomic composite material are used for adsorbing active hydrogen in the electrochemical hydrogenation reaction of the nitro-aromatic hydrocarbon, so that the reaction substrate nitro-aromatic hydrocarbon is combined with the active hydrogen to generate a target product; the copper nanowire carrier is used for selectively activating nitryl and converting nitryl into amido. Therefore, the introduction of palladium atoms in the composite material can promote the water splitting to generate active hydrogen, the conversion rate in the electroreduction reaction of the nitro-aromatic hydrocarbon is improved through the synergistic catalysis of palladium and copper sites, and meanwhile, the high selectivity and stability of the catalytic reaction are kept.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalyst preparation, and in particular relates to a copper nanowire-loaded palladium single-atom composite material, a preparation method thereof and an application thereof. Background Art

[0002] The hydrogenation of nitroaromatics to generate value-added aniline derivatives is of great significance for the production of industrial raw materials such as polyurethane (MDI) and dyes. However, the traditional thermal catalytic preparation of aniline derivatives requires the consumption of a large amount of fossil energy due to high temperature and high pressure conditions, which poses serious environmental problems. At the same time, the hydrogen required in the thermal catalytic process poses huge safety hazards in storage, transportation and reaction. Compared with thermal catalytic hydrogenation reactions, electrocatalytic hydrogenation (ECH) uses sustainable electricity as the driving energy and water as the hydrogen source, and can carry out hydrogenation reactions of unsaturated functional groups (such as carbonyl, nitro, olefins, etc.) at room temperature. Therefore, the selective hydrogenation of electrocatalytic nitroaromatics is a hot topic in current research. At present, there is an urgent need to develop efficient electrocatalytic catalysts for the selective hydrogenation of nitroaromatics to improve reaction activity and selectivity.

[0003] When other reducible groups (such as C=C, C≡C, -F / Cl / Br / I, etc.) are present in the nitroaromatic molecule, excessive hydrogenation is very likely to occur during the reduction process to generate by-products, which not only reduces the selectivity of the reaction, but also increases the difficulty of subsequent separation and purification. In addition, the complete reduction of nitroaromatics to aniline derivatives requires the avoidance of the formation of by-products such as nitrobenzene, phenylhydroxylamine, azobenzene and phenylhydrazine, while retaining other reducible groups. The literature currently reports that copper-based catalysts can reduce and replace nitro groups (to amines), C=C bonds and aromatic rings, but the copper reaction activity is low. Moreover, there are currently no reports on the use of copper-based catalysts for electrocatalytic hydrogenation. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a copper nanowire-supported palladium single-atom composite material, a preparation method thereof and an application thereof. The copper nanowire-supported palladium single-atom composite material has high catalytic efficiency, selectivity and stability for nitroaromatics in an electrochemical reduction hydrogenation reaction.

[0005] To achieve this object, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a copper nanowire-supported palladium single atom composite material, which comprises a copper nanowire carrier and a palladium single atom supported on the copper nanowire carrier;

[0007] The loading amount of palladium single atoms on the copper nanowire carrier is 0.3-1 wt %.

[0008] Preferably, the loading amount of palladium single atoms on the copper nanowire carrier is 0.4-0.85 wt %.

[0009] Preferably, the average diameter of the copper nanowire-loaded palladium single-atom composite material is 150 to 200 nm.

[0010] In a second aspect, the present invention provides a method for preparing the copper nanowire-loaded palladium single-atom composite material, comprising:

[0011] The copper nanowires are mixed with palladium salts and ion exchange is performed to obtain a copper nanowire-loaded palladium single atom composite material;

[0012] The molar ratio of the copper nanowires to the palladium salt is (75-85):1.

[0013] Preferably, the palladium salt is selected from chloropalladic acid.

[0014] Preferably, the mixing time is 20 to 60 minutes.

[0015] Preferably, the copper nanowires are prepared using a copper source as a substrate.

[0016] Preferably, the copper source is selected from copper foam and / or commercial copper flakes.

[0017] In a third aspect, the present invention provides an application of the above copper nanowire-loaded palladium single-atom composite material in the electrochemical hydrogenation reaction of nitroaromatics.

[0018] Preferably, the reference electrode in the electrochemical hydrogenation reaction is selected from a silver / silver chloride electrode.

[0019] Preferably, the counter electrode in the electrochemical hydrogenation reaction is selected from a platinum electrode.

[0020] Preferably, the potential in the electrochemical hydrogenation reaction is -0.1 V to -0.5 V relative to the standard reversible hydrogen electrode potential.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention provides a copper nanowire-supported palladium single-atom composite material, which includes a copper nanowire carrier and a palladium single atom supported on the copper nanowire carrier. The palladium atom in the copper nanowire-supported palladium single-atom composite material is used to adsorb active hydrogen in the electrochemical hydrogenation reaction of nitroaromatics, so that the reaction substrate nitroaromatics is combined with active hydrogen to generate a target product; the copper nanowire carrier has the advantages of a large specific surface area and more active sites, which is used to selectively activate the nitro group and convert the nitro group into an amine group. Therefore, the introduction of palladium atoms in the composite material can promote water splitting to produce active hydrogen, and the synergistic catalysis of palladium and copper sites increases the conversion rate in the electroreduction reaction of nitroaromatics, while maintaining the high selectivity and stability of the catalytic reaction.

[0023] In addition, the present invention controls the loading amount of palladium single atoms on the copper nanowire carrier to 0.3-1 wt%, so that palladium exists in the form of single atoms and is not easy to aggregate, so as to better play the role of adsorbing active hydrogen.

[0024] After testing, the copper nanowire-loaded palladium single-atom composite material provided by the present invention was clamped on a gold electrode clamp as a working electrode, a silver / silver chloride electrode was used as a reference electrode, and a platinum wire was used as a counter electrode. An electrochemical hydrogenation reduction reaction test was carried out, and it was found that when the relative standard hydrogen electrode potential was -0.3V, the copper nanowire-loaded palladium single-atom composite material catalyzed the conversion rate and selectivity of 3-nitrostyrene to 3-vinylaniline. Both were 100%. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a scanning electron microscope image of the copper nanowire support prepared in Example 1;

[0026] Figure 2 This is a scanning electron microscope image of the copper nanowire-supported palladium single-atom composite material prepared in Example 1;

[0027] Figure 3 This is a transmission electron microscope image of the copper nanowire-supported palladium single-atom composite material prepared in Example 1;

[0028] Figure 4 This is a high-resolution transmission electron microscopy image of the copper nanowire-loaded palladium single-atom composite material prepared in Example 1 with spherical aberration correction;

[0029] Figure 5 This is a high-angle annular dark field image-scanning transmission electron microscope image of the copper nanowire-loaded palladium single-atom composite material prepared in Example 1;

[0030] Figure 6 X-ray polycrystalline diffraction patterns of the copper nanowire carrier and the copper nanowire-supported palladium single-atom composite material prepared in Example 1;

[0031] Figure 7 X-ray photoelectron spectra of the copper nanowire carrier and the copper nanowire-supported palladium single-atom composite material prepared in Example 1;

[0032] Figure 8 X-ray absorption fine structure spectrum extended edge spectrum of palladium foil and copper foil for reference, and copper nanowire-supported palladium single-atom composite material prepared in Example 1;

[0033] Fig. 9 The conversion rates of the copper nanowire carrier and the copper nanowire-supported palladium single-atom composite material prepared in Example 1 at different potentials in the electrochemical hydrogenation reduction reaction;

[0034] Fig.10The selectivity of the copper nanowire support and the copper nanowire-supported palladium single-atom composite material prepared in Example 1 at different potentials in the electrochemical hydrogenation reduction reaction;

[0035] Fig.11 A comparison chart of conversion rate, selectivity and Faraday efficiency of the copper nanowire-supported palladium single-atom composite material prepared in Example 1 after 10 consecutive electrochemical 3-nitrostyrene reduction tests at -0.3 V relative to a standard reversible hydrogen electrode;

[0036] Fig.12 The nuclear magnetic resonance hydrogen spectra of the content of solution components of the copper nanowire-supported palladium single-atom composite material prepared in Example 1 at -0.3V relative to a standard reversible hydrogen electrode at different times;

[0037] Fig.13 The conversion rate and selectivity of the commercial palladium / carbon composite material supported on the copper foam prepared in Comparative Example 1 at different potentials in the electrochemical hydrogenation reduction reaction;

[0038] Fig.14 The mass spectrum of the electrocatalytic hydrogenation reduction of nitro groups to amine groups of the copper nanowire-supported palladium single-atom composite material prepared in Example 1;

[0039] Fig.15 The mass spectrum of the electrocatalytic hydrogenation reduction of nitro groups to amine groups when the copper nanowire-supported palladium single-atom composite material prepared in Example 1 is used as a catalyst and deuterated water is used instead of water in the cathode electrolyte;

[0040] Fig.16 This is a mass spectrum of the electrocatalytic hydrogenation reduction of nitro groups to amine groups when deuterated methanol is used instead of methanol in the cathode electrolyte using the copper nanowire-loaded palladium single-atom composite material prepared in Example 1 as a catalyst. DETAILED DESCRIPTION

[0041] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] In view of the problem in the prior art that there is an urgent need to develop a catalyst for the selective hydrogenation of nitroaromatics with high efficiency electrocatalysis to improve the reaction activity and selectivity, the present invention provides a copper nanowire-loaded palladium single-atom composite material, wherein the copper nanowire is used as a carrier to adsorb nitroaromatic substrate molecules, and the palladium single atom splits water to provide active hydrogen, which promotes the conversion of nitro groups into amine groups, thereby improving the conversion rate, reaction activity and selectivity in the electroreduction reaction of nitroaromatics.

[0043] Specifically, the present invention provides a copper nanowire-supported palladium single atom composite material, which includes a copper nanowire carrier and palladium (Pd) single atoms supported on the copper nanowire carrier.

[0044] In the present invention, the copper nanowire carrier is prepared with a copper source as a substrate, and the preparation method can refer to the technical methods commonly used by those skilled in the art. Wherein, the copper source is selected from foam copper and / or commercial copper sheet, preferably foam copper.

[0045] In the present invention, if the loading amount of the palladium atom is too low, then in the catalytic reaction system of the electrocatalytic hydrogenation reduction reaction, good catalytic activity cannot be obtained, and if the loading amount is too high, it is easy to agglomerate to form palladium nanoclusters or particles, which reduces the utilization rate of palladium, increases the catalyst cost, and also reduces the selectivity of the reaction. Therefore, the present invention is screened to control the loading amount of palladium single atoms on the copper nanowire carrier to 0.3-1wt%, specifically 0.3wt%, 0.35wt%, 0.4wt%, 0.45wt%, 0.5wt%, 0.55wt%, 0.6wt%, 0.65wt%, 0.7wt%, 0.75wt%, 0.8wt%, 0.85wt%, 0.9wt%, 0.95wt% or 1wt%, preferably 0.4-0.85wt%. Wherein, the loading amount refers to the mass percentage of the mass of the palladium element in the copper nanowire-loaded palladium single atom composite material.

[0046] In the present invention, the morphology of the copper nanowire carrier is characterized by scanning electron microscopy. Figure 1 As shown in the figure, it is a rod-like object with a certain length and a circular cross section. At the same time, scanning electron microscopy shows that the morphology of the copper nanowire carrier does not change significantly after the palladium single atom is introduced into the copper nanowire carrier (e.g. Figure 2 As shown). According to calculation and statistics, the average diameter of the copper nanowire-loaded palladium single-atom composite material is between 150 and 200 nm, and can be specifically 150 nm, 160 nm, 170 nm, 180 nm, 190 nm or 200 nm.

[0047] In addition, the transmission electron microscopy image of the copper nanowire-loaded palladium single-atom composite material ( Figure 3 ), high-resolution transmission electron microscopy images corrected for spherical aberration ( Figure 4 ) and high-angle annular dark field image-STEM image ( Figure 5 ) It can be seen that palladium atoms are uniformly dispersed on the copper nanowires and no palladium aggregation is observed.

[0048] At the same time, the X-ray polycrystal diffraction pattern of the copper nanowire-loaded palladium single-atom composite material ( Figure 6) It can be seen that there is no diffraction peak of palladium in the copper nanowire-supported palladium single-atom composite material, indicating that palladium is dispersed at the atomic level on the copper nanowire. From the X-ray absorption fine structure spectrum of the copper nanowire-supported palladium single-atom composite material ( Figure 8 ) It can be seen that there is no Pd-Pd bond in the sample, which further confirms the single-atom dispersion state of Pd.

[0049] The present invention also provides a method for preparing the copper nanowire-loaded palladium single-atom composite material, comprising the following steps:

[0050] The copper nanowires are mixed with palladium salts and ion exchange is performed to obtain a copper nanowire-loaded palladium single-atom composite material.

[0051] In the present invention, the method of introducing palladium single atoms is achieved by ion exchange, which has the advantages of mild conditions, simple and easy-to-control reactions. During the ion exchange process, palladium ions replace the lattice sites of copper in copper nanowires and are reduced to palladium atoms, and the replaced copper diffuses into the solution in the form of copper ions. The present invention can obtain a copper nanowire-loaded palladium single-atom composite material by mixing copper nanowires and palladium salts and performing ion exchange.

[0052] In some embodiments of the present invention, the copper nanowires and palladium salt are preferably mixed in a molar ratio of (75-85):1, preferably 80:1, and the mixing time is 20-60 min, preferably 30-50 min. Wherein, the mixing is preferably carried out under stirring conditions. During the above mixing process, the copper ions in the copper nanowires are ion-exchanged with the palladium ions in the palladium salt to obtain a copper nanowire-loaded palladium single-atom composite material.

[0053] In the present invention, the palladium salt is selected from chloropalladic acid.

[0054] In the present invention, the copper nanowires are prepared using a copper source as a substrate, and the preparation method can refer to the technical methods commonly used by those skilled in the art. Wherein, the copper source is selected from foam copper and / or commercial copper sheets, preferably foam copper.

[0055] In some embodiments of the present invention, the copper nanowires are preferably prepared according to the following method:

[0056] S1: mixing and reacting a copper source, an oxidant and a hydroxide to obtain copper hydroxide nanowires;

[0057] S2: calcining the copper hydroxide nanowires to obtain copper oxide nanowires; and reducing the copper oxide nanowires to obtain copper nanowires.

[0058] Wherein, the selection of the copper source is as described in the above technical solution, which will not be repeated here; the oxidant is selected from ammonium persulfate; the hydroxide is selected from sodium hydroxide and / or potassium hydroxide. In step S1, after the oxidant oxidizes the copper, the surface of the copper is oxidized and etched into copper hydroxide nanowires under the alkaline conditions of the hydroxide. In some preferred embodiments of the present invention, the copper source needs to be pretreated before use. The pretreatment is: cleaning the copper source. The cleaning is preferably: placing the copper source in ethanol, deionized water, hydrochloric acid, and deionized water for ultrasonic cleaning in sequence. The time of the ultrasonic cleaning is preferably 10 to 30 minutes, preferably 15 to 20 minutes; the concentration of hydrochloric acid is 0.1 to 0.4 mol / L, preferably 0.2 to 0.3 mol / L.

[0059] Copper hydroxide nanowires are obtained, and the copper hydroxide nanowires are calcined to obtain copper oxide nanowires. The heating rate of the calcination is 3 to 4.5°C / min, preferably 3.5 to 4°C / min; the calcination temperature is 220 to 300°C, preferably 250 to 280°C; the calcination time is 1 to 5 hours, preferably 2 to 3 hours. In the present invention, the calcination is preferably carried out in a muffle furnace.

[0060] Then, according to the present invention, the copper oxide nanowires are subjected to reduction treatment to obtain copper nanowires. The reduction treatment is: subjecting the copper oxide nanowires to an electrochemical reduction reaction. In the present invention, the potential of the electrochemical reduction reaction is -0.3 to -0.5 V relative to the standard reversible hydrogen electrode potential, preferably -0.35 to -0.4 V; the electrolyte in the electrochemical reduction reaction is selected from a neutral solution such as potassium sulfate solution, phosphate buffer, potassium chloride, etc.; the time of the electrochemical reduction reaction is 0.5 to 3 hours, preferably 1 to 2 hours.

[0061] In summary, in some embodiments of the present invention, the preparation method of the copper nanowire-supported palladium single-atom composite material comprises the following steps:

[0062] (1) ultrasonically cleaning the copper foam in ethanol, deionized water, hydrochloric acid, and deionized water in sequence;

[0063] (2) placing the cleaned copper foam in an ammonium persulfate and sodium hydroxide solution to obtain copper hydroxide nanowires;

[0064] (3) calcining the copper hydroxide nanowires to obtain copper oxide nanowires;

[0065] (4) electroreducing the copper oxide nanowires into copper nanowires in a potassium sulfate solution;

[0066] (5) Immersing the copper nanowires in a chloropalladic acid solution for ion exchange to obtain a copper nanowire-loaded palladium single atom composite material.

[0067] Specifically, the present invention first cuts the foam copper and sequentially places it in ethanol, deionized water, hydrochloric acid with a concentration of 0.2 mol / L, and deionized water for ultrasonic cleaning for 15 minutes; then, the cleaned foam copper is placed in a mixed solution containing 0.1 mol / L ammonium persulfate and 2.5 mol / L sodium hydroxide for 20 minutes to grow nanowires; then, the copper hydroxide nanowires are calcined in an air atmosphere to obtain copper oxide nanowires, and the calcination temperature is 250°C, the heating rate is 4°C / min, and the time is 2 hours; then, the copper oxide nanowires are electro-reduced in a potassium sulfate solution with a concentration of 0.5 mol / L and a relative standard reversible hydrogen electrode of -0.4V for 1 hour to obtain copper nanowires; finally, the copper nanowires are placed in a 0.05 mmol / L chloropalladic acid solution and immersed for 30 minutes to finally obtain a copper nanowire-loaded palladium single-atom composite material.

[0068] The preparation method provided by the present invention is simple, convenient, easy to implement, conducive to industrialization or industrial production, and has great practical significance.

[0069] The present invention also provides an application of the copper nanowire-supported palladium single-atom composite material involved in the above technical solution in the electrochemical hydrogenation reaction of nitroaromatics. Wherein, the cathode electrolyte is a mixture of lithium perchlorate solution and methanol (volume ratio is 1:1), the anode electrolyte is a lithium perchlorate solution, and the reaction catalyst is the copper nanowire-supported palladium single-atom composite material involved in the above technical solution. In the electrochemical hydrogenation reaction, nitroaromatics are reduced to aniline derivatives.

[0070] It should be noted that the electrochemical nitro reduction reaction to amino group is a complex process of six electron transfer, which generally follows the traditional adsorption evolution mechanism. In the present invention, the reaction substrate nitroaromatic is first adsorbed on the copper nanowire-supported palladium single atom composite material, and then the reaction substrate nitroaromatic combines with the active hydrogen generated by water dissociation under electrochemical conditions on the copper nanowire-supported palladium single atom composite material, and finally generates aniline derivatives, which are then desorbed.

[0071] The copper nanowire-loaded palladium single-atom composite material provided by the present invention is clamped on a gold electrode clamp as a working electrode, a silver / silver chloride electrode is used as a reference electrode, and a platinum wire is used as a counter electrode to conduct an electrochemical hydrogenation reduction reaction test, wherein the potential in the electrochemical hydrogenation reaction is -0.1v to -0.5v relative to the standard reversible hydrogen electrode potential. The results show that in the electrochemical reduction reaction of 3-nitrostyrene to 3-vinylaniline, as the relative standard hydrogen electrode potential becomes more negative, the reaction conversion rate of a single copper nanowire and a copper nanowire-loaded palladium single-atom composite material gradually increases, while the selectivity gradually decreases; when the relative standard hydrogen electrode potential is -0.3V, the conversion rates of 3-nitrostyrene to 3-vinylaniline of a single copper nanowire and a copper nanowire-loaded palladium single-atom composite material are 78.95% and 100%, respectively, and the selectivity is 100%. It should be noted that the reference electrode may also be selected from other reference electrodes commonly used by those skilled in the art, as long as the corresponding relative standard reversible hydrogen electrode potential remains unchanged. At the same time, different reference electrodes have different voltages input into the instrument while ensuring the same relative standard reversible hydrogen electrode potential.

[0072] In addition, the present invention further conducted a constant voltage test on the copper nanowire-loaded palladium single-atom composite material for 10 consecutive times for 2 hours at a relative standard hydrogen electrode of -0.3 V, and found that the conversion rate and selectivity of 3-nitrostyrene were still 100%, and the Faraday efficiency was maintained above 65%, indicating that the copper nanowire-loaded palladium single-atom composite material has high catalytic stability.

[0073] The above results indicate that the palladium and copper sites present in the copper nanowire-loaded palladium single-atom composite material provided by the present invention synergistically catalyze and improve the conversion rate in the electroreduction reaction of nitroaromatics while maintaining the high selectivity and stability of the catalytic reaction.

[0074] In order to further illustrate the present invention, the following examples are used to explain it in detail. The experimental raw materials used in the following examples of the present invention are all common commercial products. Among them, the foam copper was purchased from Xingzhenghong Technology Enterprise Store, with a specification of 200*300*1.0mm and a pore density of 130ppi.

[0075] Example 1

[0076] This embodiment provides a copper nanowire-supported palladium single-atom composite material with an average diameter of 150 to 200 nm. The synthesis method thereof is as follows:

[0077] (1) Cut the 5×5cm 2The copper foam was ultrasonically cleaned in ethanol for 15 minutes, and then the cleaned copper foam was ultrasonically cleaned in deionized water for 15 minutes, and then the cleaned copper foam was ultrasonically cleaned in 250mL of 0.2mol / L hydrochloric acid for 15 minutes, and finally ultrasonically cleaned in deionized water for 15 minutes;

[0078] (2) Dissolve 25 g of sodium hydroxide in 250 mL of deionized water, and add 5.7 g of ammonium persulfate to the solution after the solution cools to room temperature. After the solution is completely dissolved, place the cleaned copper foam in the solution, seal the beaker with plastic wrap, and let it stand for 20 minutes. After blue copper hydroxide nanowires grow on the surface of the copper foam, take out the copper foam, wash it, and dry it in an oven at 60° C. for 3 hours.

[0079] (3) calcining the copper hydroxide nanowires in a muffle furnace at a heating rate of 4°C / min, a calcination temperature of 250°C, and a calcination time of 2 hours to obtain black copper oxide nanowires. The copper oxide nanowires were subjected to an electrochemical reduction reaction in an electrolytic cell containing 200 mL of a 0.5 mol / L potassium sulfate electrolyte, with an overpotential of -0.4 V relative to a standard reversible hydrogen electrode potential applied by an electrochemical workstation, and a reduction time of 1 hour to finally obtain a copper nanowire carrier;

[0080] (4) 88.7 mg of palladium chloride was placed in 0.0833 mL of concentrated hydrochloric acid and ultrasonically dissolved in a 1.5 mL centrifuge tube. The palladium chloride was first dissolved with concentrated hydrochloric acid, and the solution was transferred to a 20 mL glass vial and diluted to 10 mL with 9.917 mL of deionized water to obtain a 50 mmol / L chloropalladium acid solution; 250 μL of the chloropalladium acid solution was taken out and diluted to 250 mL of deionized water to obtain a 0.05 mmol / L chloropalladium acid solution; finally, the copper nanowire carrier was placed in the solution and stirred for 30 minutes to obtain a copper nanowire-loaded palladium single atom composite material.

[0081] The copper nanowire-loaded palladium single-atom composite material was cut into 4 small pieces and placed in a 50mL small glass bottle. Ethanol was added for 4 hours of ultrasound. After every 1 hour of ultrasound, the ethanol was poured into a centrifuge tube and new ethanol was added to the 50mL small glass bottle to continue ultrasound. Finally, all the ethanol in the centrifuge tube was centrifuged at 10000rpm for 3min. After washing with ethanol 3 times and deionized water 3 times, vacuum freeze-dried for 48h. Take 5mg of freeze-dried copper nanowire-loaded palladium single-atom particles and dissolve them in 1mL of aqua regia. After complete dissolution, add 1.5mL of deionized water and dilute to 2.5mL for inductively coupled plasma atomic emission spectroscopy to test the concentration of palladium in the solution. The test result was 17mg / L. Therefore, the mass of palladium in the 5mg freeze-dried copper nanowire-loaded palladium single-atom particles is 0.0425mg, and the loading amount of palladium is 0.85wt%.

[0082] The scanning electron microscope image of the copper nanowire carrier prepared in this example is as follows: Figure 1 As shown, the scanning electron microscope images, transmission electron microscope images, spherical aberration corrected high-resolution transmission electron microscope images and high-angle annular dark field image-scanning transmission electron microscope images of the copper nanowire-loaded palladium single-atom composite material are shown in Figure 1. Figures 2 to 5 As shown. Figure 1 It can be seen that the grown copper nanowires are evenly distributed, and their average diameter is measured to be 150-200 nm. Figure 2 Copper nanowire-supported palladium single-atom composites and Figure 1 The morphology of the single copper nanowire carrier in the experiment has not changed much, indicating that the introduction of single palladium atoms has no significant effect on the morphology of the copper nanowire carrier. Figure 3 and 4 It can be seen that palladium is evenly dispersed on the copper nanowires without obvious aggregation. Figure 5 It can be seen that the palladium atoms are uniformly dispersed on the copper nanowire support and no palladium aggregation is observed, which is consistent with Figures 3-4 Be consistent.

[0083] The X-ray polycrystalline diffraction patterns of the copper nanowire carrier and the copper nanowire-loaded palladium single-atom composite material prepared in this example are as follows: Figure 6 As shown, it can be seen that both the copper nanowire-loaded palladium single atom composite material and the copper nanowire support show diffraction peaks of copper, and there is no diffraction peak of palladium in the copper nanowire-loaded palladium single atom composite material, which proves the atomic-level dispersion of palladium.

[0084] The X-ray photoelectron spectra of the copper nanowire carrier and the copper nanowire-loaded palladium single-atom composite material prepared in this example are shown in FIG. Figure 7 As shown, the peaks of the copper nanowire-loaded palladium single-atom composite material and the copper nanowire carrier are the same, indicating that the valence state of the copper species in the copper nanowire-loaded palladium single-atom composite material is the same as the valence state of the copper species in the copper nanowire carrier, both of which are metallic copper.

[0085] The X-ray absorption fine structure spectrum extended edge spectra of the copper nanowire-supported palladium single atom composite material prepared in this embodiment, the reference palladium foil and the copper foil are shown in FIG. Figure 8 As shown, it can be seen that no Pd-Pd bonds appear in the copper nanowire-supported palladium single atom composite material, confirming the monodisperse state of Pd.

[0086] Example 2

[0087] (1) Referring to the method of Example 1, a copper foam is provided;

[0088] (2) Dissolve 35 g of potassium hydroxide in 250 mL of deionized water, and add 5.7 g of ammonium persulfate to the solution after the solution cools to room temperature. After the solution is completely dissolved, place the cleaned copper foam in the solution, seal the beaker with plastic wrap, and let it stand for 20 minutes. After blue copper hydroxide nanowires grow on the surface of the copper foam, take out the copper foam, wash it, and dry it in a 50° C. oven for 3 hours;

[0089] (3) calcining the copper hydroxide nanowires in a muffle furnace at a heating rate of 3.5°C / min, a calcination temperature of 250°C, and a calcination time of 2 hours to obtain black copper oxide nanowires. The copper oxide nanowires were subjected to an electrochemical reduction reaction in an electrolytic cell containing 200 mL of 0.5 mol / L phosphate buffer, with an overpotential of -0.35 V relative to a standard reversible hydrogen electrode potential applied by an electrochemical workstation, and a reduction time of 2 hours to finally obtain a copper nanowire carrier;

[0090] (4) Referring to the method of Example 1, 125 μL of the prepared 50 mmol / L chloropalladic acid solution was taken out and diluted into 250 mL of deionized water to obtain a 0.025 mmol / L chloropalladic acid solution; finally, the copper nanowire carrier was placed in the solution and stirred for 30 minutes to obtain a copper nanowire-loaded palladium single-atom composite material.

[0091] The copper nanowire-loaded palladium single-atom composite material was cut into 4 small pieces and placed in a 50mL small glass bottle. Ethanol was added for 4 hours of ultrasound. After every 1 hour of ultrasound, the ethanol was poured into a centrifuge tube and new ethanol was added to the 50mL small glass bottle to continue ultrasound. Finally, all the ethanol in the centrifuge tube was centrifuged at 10000rpm for 3min. After washing with ethanol 3 times and deionized water 3 times, vacuum freeze-dried for 48h. 6mg of freeze-dried copper nanowire-loaded palladium single-atom particles were dissolved in 1mL of aqua regia. After complete dissolution, 1.5mL of deionized water was added to dilute to 2.5mL for inductively coupled plasma atomic emission spectroscopy to test the concentration of palladium in the solution. The test result was 7.2mg / L. Therefore, the mass of palladium in the 6mg freeze-dried copper nanowire-loaded palladium single-atom particles is 0.018mg, and the loading amount of palladium is 0.3wt%.

[0092] Example 3

[0093] (1) Referring to the method of Example 1, a copper foam is provided;

[0094] (2) Dissolve 30 g of sodium hydroxide in 300 mL of deionized water, and add 6.846 g of ammonium persulfate to the solution after the solution cools to room temperature. After the solution is completely dissolved, place the cleaned copper foam in the solution, seal the beaker with plastic wrap, and let it stand for 25 minutes. After blue copper hydroxide nanowires grow on the surface of the copper foam, take out the copper foam, wash it, and dry it in an oven at 55° C. for 3 hours.

[0095] (3) calcining the copper hydroxide nanowires in a muffle furnace at a heating rate of 4°C / min, a calcination temperature of 250°C, and a calcination time of 2 hours to obtain black copper oxide nanowires. The copper oxide nanowires were subjected to an electrochemical reduction reaction in an electrolytic cell containing 200 mL of 0.5 mol / L phosphate buffer, with an overpotential of -0.45 V relative to a standard reversible hydrogen electrode potential applied by an electrochemical workstation, and a reduction time of 2 hours to finally obtain a copper nanowire carrier;

[0096] (4) Referring to the method of Example 1, 300 μL of the prepared 50 mmol / L chloropalladic acid solution was taken out and diluted into 250 mL of deionized water to obtain a 0.06 mmol / L chloropalladic acid solution; finally, the copper nanowire carrier was placed in the solution and stirred for 30 minutes to obtain a copper nanowire-loaded palladium single atom composite material.

[0097] The copper nanowire-loaded palladium single-atom composite material was cut into 4 small pieces and placed in a 50mL small glass bottle. Ethanol was added for 4 hours of ultrasound. After every 1 hour of ultrasound, the ethanol was poured into a centrifuge tube and new ethanol was added to the 50mL small glass bottle to continue ultrasound. Finally, all the ethanol in the centrifuge tube was centrifuged at 10000rpm for 3min. After washing with ethanol 3 times and deionized water 3 times, vacuum freeze-dried for 48h. 6.5mg of freeze-dried copper nanowire-loaded palladium single-atom particles were dissolved in 1mL of aqua regia. After complete dissolution, 1.5mL of deionized water was added to dilute to 2.5mL for inductively coupled plasma atomic emission spectroscopy to test the concentration of palladium in the solution. The test result was 26mg / L. Therefore, the mass of palladium in the 6.5mg freeze-dried copper nanowire-loaded palladium single-atom particles is 0.065mg, and the loading amount of palladium is 1wt%.

[0098] Comparative Example 1

[0099] 2.66 mg of commercial palladium / carbon with a palladium mass fraction of 10% and 40 μL of Nafion solution with a mass fraction of 5% were dispersed in a mixed solution of 660 μL of ethanol and 300 μL of deionized water, and ultrasonicated for 20 minutes to obtain a uniform solution; then, the above solution was evenly dropped on a 1×2.5 cm 2 Take 1×2.5cm 2 The above copper foam loaded with commercial palladium / carbon composite material was used as the working electrode.

[0100] Performance Testing

[0101] 1. Electrocatalysts and electrochemical hydrogenation reduction reaction tests of copper nanowire-supported palladium single atom composites and copper foam-supported commercial palladium / carbon composites as active ingredients

[0102] The 5×5 cm 2 The copper nanowire-loaded palladium single-atom composite material was cut into 10 pieces of 1×2.5 cm 2 Then, take one piece of 1×2.5cm 2 Copper nanowires loaded with palladium single atom composite materials or 1×2.5cm 2 The above-mentioned copper foam loaded commercial palladium / carbon composite material is clamped on a gold electrode clamp as a working electrode, a silver / silver chloride electrode is used as a reference electrode, and a platinum wire is used as a counter electrode; before electrochemical hydrogenation reduction, it should be reduced in an electrolytic cell containing 100mL of 0.5mol / L potassium sulfate electrolyte for 20 minutes, and the reduction condition is that the relative standard reversible hydrogen electrode potential is -0.4V; after reduction, the surface of the copper nanowire-loaded palladium single-atom composite material is cleaned and an electrochemical hydrogenation reduction reaction is carried out in an H-type electrolytic cell, the anode cell is filled with 30mL of 0.15mol / L lithium perchlorate, the cathode cell is filled with 30mL (methanol and lithium perchlorate solution volume ratio is 1:1) 0.15mol / L lithium perchlorate solution and 5mmol / L 3-nitrostyrene, the stirring speed is 500rpm, the anode cell and the cathode cell are separated by a proton exchange membrane of model Nafion-117, and the reaction potential is applied externally through an electrochemical workstation.

[0103] 2. Conversion rate and selectivity test of copper nanowire-supported palladium single-atom composite materials in electrochemical hydrogenation reduction reaction

[0104] Under the reaction conditions of the above electrochemical hydrogenation reduction reaction test, a constant voltage test was adopted; the voltage range relative to the standard hydrogen electrode was set to -0.1V to -0.5V, and the reaction time was 1.75h. After the test was completed, 400μL of the solution was taken out from the cathode cell electrolyte and injected into the nuclear magnetic resonance tube, and 100μL of dimethyl sulfoxide and 50μL of tetramethylsilane were added and mixed evenly for nuclear magnetic resonance hydrogen spectrum test.

[0105] The conversion rate and selectivity of the copper nanowire-supported palladium single-atom composite material and the copper nanowire carrier prepared in Example 1 within the set voltage range are as follows: Fig. 9 and 10 As shown. Fig. 9 , 10It can be seen that the electrochemical hydrogenation reduction activity of 3-nitrostyrene of copper nanowire-loaded palladium single-atom composite material is far superior to that of simple copper nanowire carrier. As the potential relative to the standard hydrogen electrode becomes more negative, the reaction conversion rate of copper nanowire carrier and copper nanowire-loaded palladium single-atom composite material gradually increases, while the selectivity gradually decreases. When the potential is low, such as -0.2V relative to the standard hydrogen electrode, the conversion rates of copper nanowire-loaded palladium single-atom composite material and copper nanowire carrier are both less than 100%, 95.86% and 56.95% respectively. When the potential reaches -0.3V relative to the standard hydrogen electrode, the conversion rate of copper nanowire-loaded palladium single-atom composite material can just reach 100%, which is 1.26 times that of a single copper nanowire carrier, and the selectivity also reaches 100%; when the potential is more negative, such as -0.4V relative to the standard hydrogen electrode, the conversion rates of copper nanowire-loaded palladium single-atom composite material and single copper nanowire carrier are 100% and 96% respectively, while the selectivity is less than 100%, 95.42% and 98.24% respectively. Fig.11 As shown, when the relative voltage of the standard hydrogen electrode is -0.3V, the copper nanowire-supported palladium single-atom composite material is subjected to 10 consecutive constant voltage tests for 2 hours, and the conversion rate and selectivity of 3-nitrostyrene are still 100%, and the Faraday efficiency is maintained above 65%, indicating that the copper nanowire-supported palladium single-atom composite material provided by the present invention has high catalytic stability. Fig.12 As shown, the electrocatalytic 3-nitrostyrene reduction test was carried out at -0.3 V relative to the standard hydrogen electrode. With the increase of reaction time, the concentration of 3-nitrostyrene gradually decreased, the peak area of ​​its nuclear magnetic resonance hydrogen spectrum also gradually decreased, while the peak area of ​​the product 3-vinylaniline gradually increased. After 2 hours of reaction, 3-nitrostyrene was completely converted into 3-vinylaniline, but not into 3-ethylaniline.

[0106] The conversion rate of the commercial palladium / carbon composite material supported by the foam copper prepared in Comparative Example 1 within the set voltage range is as follows: Fig.13 As shown, it can be seen that the activity and intrinsic activity of the commercial palladium / carbon composite material supported on foam copper as an electrochemical catalyst for electrocatalytic hydrogenation reduction reaction are much lower than the copper nanowire-supported palladium single atom composite material provided by the present invention.

[0107] 3. Conversion rate and selectivity test of copper nanowire-supported palladium single-atom composite materials for different nitroaromatic substrates in electrochemical hydrogenation reduction reaction

[0108] Under the reaction conditions of the above electrochemical hydrogenation reduction reaction test, a constant voltage test was adopted, each reaction time was 2 hours, and the voltage was set to be maintained at -0.3 V relative to the standard hydrogen electrode. The copper nanowire-supported palladium single-atom composite material was subjected to a 2-hour constant voltage test on different nitroaromatic substrates at this voltage. As shown in Table 1, the conversion rates of different nitroaromatic substrates were all 100%, and the selectivity was also above 80%, indicating that the copper nanowire-supported palladium single-atom composite material provided by the present invention exhibits good catalytic performance for the selective hydrogenation of the nitro group of nitroaromatics.

[0109] Table 1

[0110]

[0111] 4. Deuterated water was used instead of deionized water and deuterated methanol was used instead of methanol in the electrochemical hydrogenation reduction reaction of copper nanowire-supported palladium single-atom composites to verify the source of active hydrogen

[0112] Under the reaction conditions of the above electrochemical hydrogenation reduction test, a constant voltage test was adopted, the voltage relative to the standard hydrogen electrode was set to -0.3V, and the reaction time was 2h. After the reaction was completed, the cathode pool electrolyte was taken out, 10mL of dichloromethane was added, and the mixture was shaken for 30s, and then left to stand for half an hour until the solution was completely separated. After the above solution was extracted, 5mL of the lower dichloromethane solvent was taken out and tested by gas chromatography-mass spectrometry. The results are as follows Fig.14 , 15 and 16.

[0113] like Fig.14 As shown, the mass-to-charge ratio of 3-nitrostyrene after electrocatalytic hydrogenation reduction to 3-vinylaniline is 119; Fig.15 As shown in the figure, when deuterium water replaces water in the electrolyte, the mass-to-charge ratio of the test result becomes 121; Fig.16 As shown, when deuterated methanol replaces methanol in the electrolyte, the mass-to-charge ratio is still 119, so the active hydrogen required for the electrocatalytic hydrogenation reduction of nitro groups to amine groups comes from water.

[0114] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A copper nanowire-loaded palladium single-atom composite material, It is characterized in that It includes a copper nanowire support and a palladium single atom supported on the copper nanowire support; The loading amount of palladium single atoms on the copper nanowire carrier is 0.3-1 wt %.

2. The copper nanowire-supported palladium single-atom composite material according to claim 1, It is characterized in that The loading amount of palladium single atoms on the copper nanowire carrier is 0.4-0.85 wt %.

3. The copper nanowire-supported palladium single-atom composite material according to claim 1 or 2, It is characterized in that The average diameter of the copper nanowire-loaded palladium single-atom composite material is 150-200 nm.

4. A method for preparing a copper nanowire-supported palladium single-atom composite material according to any one of claims 1 to 3, It is characterized in that include: The copper nanowires are mixed with palladium salts and ion exchange is performed to obtain a copper nanowire-loaded palladium single atom composite material; The molar ratio of the copper nanowires to the palladium salt is (75-85):

1.

5. The preparation method according to claim 4, It is characterized in that The palladium salt is selected from chloropalladic acid.

6. The preparation method according to claim 4 or 5, It is characterized in that The mixing time is 20 to 60 minutes.

7. The preparation method according to any one of claims 4 to 6, It is characterized in that The copper nanowires are prepared using a copper source as a substrate; The copper source is selected from copper foam and / or commercial copper flakes.

8. Use of the copper nanowire-supported palladium single-atom composite material according to any one of claims 1 to 3 or the copper nanowire-supported palladium single-atom composite material prepared by the preparation method according to any one of claims 4 to 7 in the electrochemical hydrogenation reaction of nitroaromatics.

9. The use according to claim 8, It is characterized in that The reference electrode in the electrochemical hydrogenation reaction is selected from a silver / silver chloride electrode; The counter electrode in the electrochemical hydrogenation reaction is selected from a platinum electrode.

10. The use according to claim 8 or 9, It is characterized in that The potential in the electrochemical hydrogenation reaction is -0.1V to -0.5V relative to the standard reversible hydrogen electrode potential.