Copper foil preparation method for improving wrinkle problem and preparation method of lithium secondary battery comprising copper foil
By using organic composite electrolyte additives in lithium secondary batteries, the wrinkles and belt breakage problems caused by the reduction of copper foil thickness are solved, the capacity and stability of lithium secondary batteries are improved, and high efficiency is achieved Improved battery performance and safety.
Patent Information
- Application Number
- CN202411002176.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In lithium secondary batteries, the decrease in the thickness of copper foil leads to wrinkles and broken belt defects, affecting production efficiency and battery capacity stability. In addition, the volume expansion of high-capacity metals or composite materials during charging and discharging, increasing the expansion of copper foil Tensile force requirements.
Using organic composite electrolyte additives, including brighteners, locating agents and leveling agents, copper sulfate electrolyte is prepared by electrolysis, controlling the grain orientation of the copper layer, reducing residual stress, reducing the probability of defects, and preparing high tensile strength and extension The copper foil is used in lithium secondary batteries to prevent wrinkles and strip breakage.
A copper foil with a thickness of 4-10μm, a weight deviation of ≤3%, and a tensile strength of 30-50kgf/mm2 was realized, which suppressed the wrinkles and belt breakage of lithium secondary batteries during the charging and discharge cycle, and improved the battery energy density. and safety, reducing manufacturing costs.
Smart Images

Figure CN118932436A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper foil, and in particular to a method for preparing a copper foil with improved wrinkle problems and a method for preparing a lithium secondary battery comprising the copper foil. Background Art
[0002] Secondary batteries use the reversibility of chemical reactions to convert a chemical reaction into electrical energy to generate electricity; they can also convert electrical energy into chemical energy for storage, and can be used as an energy converter, also known as "rechargeable batteries." Among secondary batteries, lithium secondary batteries are widely used in electric vehicles, 3C digital products, and energy storage fields due to their high energy density, long cycle life, and low self-discharge. With the proposal of the "carbon peak" and "carbon neutrality" goals, the comprehensive green transformation of economic and social development is being promoted. While new energy vehicles and energy storage systems are developing rapidly, the demand for lithium secondary batteries is also increasing rapidly.
[0003] The composition of lithium secondary batteries mainly includes five parts: active materials, current collectors, diaphragms, electrolytes and shells. Electrolytic copper foil is the only choice for negative current collectors of lithium secondary batteries because of its soft texture, good conductivity and low price. The increase in demand for lithium secondary batteries not only increases the need for high-capacity and high-quality secondary batteries, but also puts forward higher requirements for negative current collector copper foil that can improve the characteristics of lithium secondary batteries, that is, it is necessary to give lithium secondary batteries high capacity and stably maintain the capacity of copper foil. At present, there are two developments in copper foil. One is to develop in the direction of thinner thickness, and the other is to develop high-performance composite copper foil. The common point of the two development directions is the reduction of copper foil thickness. The reduction in copper foil thickness causes copper foil to be prone to wrinkles or broken belts during production and preparation, lithium secondary battery process and use, which is unfavorable to copper foil production efficiency and lithium secondary battery capacity and stability. Therefore, the development of ultra-thin copper foil must first improve the wrinkle problem of copper foil for lithium secondary battery current collector.
[0004] As the thickness of the copper foil decreases, the amount of active material applied during the coating process also increases, thereby increasing the capacity of the secondary battery, but in the subsequent rolling process, the probability of broken belts and wrinkles increases. In addition, in order to increase the capacity of lithium secondary batteries, high-capacity metals or composite materials have also been developed for use as active materials. Since metal materials and composite materials expand severely in volume during charging and discharging, copper foil needs to withstand greater expansion and stretching forces, so the current collector copper foil must also have excellent physical properties such as tensile strength and elongation. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a copper foil with improved wrinkle problem, comprising the following steps:
[0006] S1, preparing copper sulfate electrolyte;
[0007] S2, adding hydrochloric acid and an organic composite electrolyte additive, wherein the organic composite electrolyte additive includes a brightener, a positioning agent, and a leveling agent;
[0008] S3, electrolytically preparing raw foil, including electrolyzing raw foil under the conditions of a preset electrolyte temperature and a preset current density, wherein the preset electrolyte temperature is 40-60° C., and the preset current density is 3500 A / m 2 -6000 A / m 2 ;
[0009] S4, performing anti-oxidation treatment on the surface of the electrolytic foil;
[0010] S5, rolling, aging and slitting the raw foil into finished foil.
[0011] The use of organic composite additives to improve the rigidity of copper foil has a stronger leveling effect. By controlling the grain orientation of the copper layer, the residual stress in the foil is reduced, the probability of product defects is reduced, and curling, wrinkling and breaking of the copper foil during manufacturing and use are prevented.
[0012] Preferably, the preparation of the copper sulfate electrolyte comprises first adding copper raw materials such as copper wire with a purity of ≥99.9% and a diameter of 3-8 mm, copper plate with a purity of ≥99.9% in a ratio of 1:1 or 1:2 into a copper dissolving tank together with sulfuric acid and deionized water, and using a screw fan to pass high-temperature steam to cause an oxidation reaction between copper and sulfuric acid to generate a copper sulfate electrolyte, and then filtering through a diatomaceous earth filter, a security filter, and a precision filter to obtain a pure copper sulfate electrolyte.
[0013] Preferably, the copper ion concentration in the copper sulfate aqueous solution is 70-90 g / L, and the sulfuric acid content is 100-120 g / L.
[0014] Preferably, the hydrochloric acid is prepared by adding a 36%-38% hydrogen chloride solution into deionized water to prepare a 0.25%-0.5% hydrogen chloride aqueous solution.
[0015] Preferably, the brightener includes sulfonic acid and its metal salt, including sodium polydisulfide propane sulfonate (SPS), sodium methylene dinaphthalene sulfonate, SH-110 sodium thiazoline disulfide propane sulfonate, or a mixture of two or more thereof. The brightener has both brightening and leveling effects, and inhibits defects generated during copper foil deposition. The added concentration range is 10-150ppm.
[0016] The moving agent includes at least one of polyethylene glycol (PEG) and polypropylene glycol (PPG), wherein the relative molecular weight of polyethylene glycol (PEG) is 3000-6000, and the moving agent is a macromolecular additive, which blocks the diffusion of copper ions near the cathode, inhibits the electrodeposition of copper, and makes the copper foil more dispersed and flat. The added concentration range is 10-50ppm;
[0017] The leveling agent includes at least one of unsaturated organic sulfides or nitrides, including thiourea, 1,2-ethylenethiourea, 2-mercaptobenzimidazole, 2-mercaptobenzothiazole, benzotriazole, one or a mixture of two or more thereof. The leveling agent is adsorbed on the protruding points on the surface of the copper foil through mutual interaction, promotes the electrodeposition of the concave parts of the copper foil, and plays a leveling role. The added concentration range is 5-50ppm;
[0018] Preferably, the hydrochloric acid is added to the electrolyte to provide Cl - , as a copper foil additive, the added concentration range is 18-40ppm, which plays a role of cathode depolarization in the electrodeposition process and promotes the deposition of copper; the preset electrolysis temperature of the electrolyte is 40-60°C, and the preset current density is 3500A / m 2 -6000A / m 2 , the copper sulfate electrolyte flow rate is 30-50m3 / h.
[0019] Preferably, the finished foil has a thickness of 4-10 μm, a weight deviation of ≤3%, and a tensile strength of 30-50 kgf / mm 2 , elongation ≥ 4%, and it has a bright surface and a matte surface, and the differences in Rz and Ra of the bright / matte surfaces are ≤ 0.5μm and 0.06μm respectively.
[0020] Preferably, the finished foil has multiple oriented crystal planes, wherein the sum of the texture coefficients TC of the (111) plane and the (200) plane accounts for 30%-60% of the sum of the texture coefficients TC of the (111) plane, the (200) plane and the (220) plane, and can be used as copper foil for lithium secondary battery current collector.
[0021] The present invention also provides a method for preparing a lithium secondary battery containing copper foil with improved wrinkle problem, and the specific steps are as follows:
[0022] Step 1: Preparation of negative electrode for lithium secondary battery: 90-98 parts by weight of commercially available graphite negative electrode as negative electrode active material, mixed with 0.5-2 parts of conductive carbon black, 0.5-1.5 parts of styrene-butadiene rubber (SBR), 0.5-1.5 parts of carboxymethyl cellulose (CMC) and 190-230 parts of deionized water to obtain negative electrode slurry, which is then coated on copper foil, dried, and rolled into a negative electrode sheet;
[0023] Step 2: Place the positive electrode sheet, negative electrode sheet, separator and electrolyte in an aluminum shell to make a square lithium secondary battery.
[0024] Preferably, a 32 cm wide, 60 μm thick slurry is applied to both sides of the copper foil using a scraper, dried at 120°C, and heated at 1.0 t / cm 2 Pressing under pressure to form a negative electrode sheet;
[0025] After the square lithium secondary battery was made, it was charged at a voltage of 4.2V and discharged at a voltage of 3.2V, with a charge and discharge rate of 1C at room temperature, and was cycled 300 times.
[0026] Compared with the prior art, the invention has the following beneficial effects: the invention can produce a product with a thickness of 4-10 μm, a weight deviation of ≤3%, and a tensile strength of 30-50 kgf / mm 2 , copper foil for lithium secondary battery current collector with elongation ≥4%. Secondly, the copper foil prepared by organic composite addition has a bright surface and a matte surface, and the difference between the light / matte surface Rz and Ra is ≤0.5μm and 0.06μm respectively. The copper foil has multiple oriented crystal planes, among which the sum of the texture coefficients TC of the (111) plane and the (200) plane accounts for 30%-60% of the sum of the texture coefficients TC of the (111) plane, the (200) plane and the (220) plane, and has a stronger ability to inhibit the generation and diffusion of defects. In addition, the lithium secondary battery using the copper foil as the negative electrode current collector did not show any wrinkles or broken belts during the battery cell process and after 300 charge and discharge cycles at 1C rate at room temperature. While improving the energy density of the lithium secondary battery, it reduces the manufacturing cost of the battery and improves the safety and reliability of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is an EBSD photograph of a 6 μm thick copper foil prepared in Example 2 of the present invention;
[0028] Figure 2 XRD spectrum of the 6 μm copper foil prepared in Example 1-8 (corresponding to Sample 1-8) of the present invention;
[0029] Figure 3 This is a schematic diagram of a square lithium secondary battery negative electrode sheet (after rolling) prepared in the present invention.
[0030] In the figure: 0—copper foil; 1-1 / 1-2—anti-oxidation layer; 2-1 / 2-2—active material layer. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0032] Example 1: Copper raw materials such as copper wire with a purity of ≥99.9%, copper plate with a purity of ≥99.9%, etc. are added to a copper dissolving tank in a ratio of 1:1 together with sulfuric acid and deionized water. Under the condition of high-temperature steam introduced by a screw fan, copper and sulfuric acid undergo oxidation reaction to generate copper sulfate electrolyte. After three-stage filtration through a diatomaceous earth filter, a security filter, and a precision filter, a pure copper sulfate electrolyte is obtained. Subsequently, hydrochloric acid and an organic composite electrolyte additive are added. The copper ion concentration in the copper sulfate aqueous solution is 90g / L, and the sulfuric acid content is 105g / L. The flow rate is 45m 3 / h, the electrolyte with a temperature of 55℃ is transported to the foil machine, and the current density is 5500A / m 2 , produce 6μm copper foil, the raw foil is anti-oxidation treated, rolled, aged and slit to obtain the finished foil.
[0033] The hydrochloric acid is prepared into the electrolyte tank. - The concentration is 23 mg / L. The composite additive uses SPS (component A) with a concentration of 80 ppm; PEG with a molecular weight of 5000 (component B) with a concentration of 40 ppm; a mixture of 1,2-ethylene thiourea and 2-mercaptobenzothiazole in a ratio of 2:1 (component C) with a concentration of 40 ppm.
[0034] Three rolls of 800m copper foil were produced in batches. The raw foil samples were taken for testing. After baking at 150℃ for 10 minutes, the average tensile strength was measured to be 42.8kgf / mm 2 , weight deviation is 1.7% and average elongation is 8.1%.
[0035] The copper foil was used as the negative electrode current collector of the lithium secondary battery. By weight, 96 parts of commercially available graphite negative electrode were used as the negative electrode active material, mixed with 2 parts of conductive carbon black, 1 part of styrene-butadiene rubber (SBR), 1 part of carboxymethyl cellulose (CMC) and 220 parts of deionized water to obtain a negative electrode slurry. A scraper was used to apply a 32 cm wide, 60 μm thick slurry on both sides of the copper foil, dried at 120°C, and heated at 1.0 t / cm 2 The negative electrode was pressed under pressure; and placed in an aluminum shell with the positive electrode, separator and electrolyte to make a 5PCS square lithium secondary battery. The battery was charged at a voltage of 4.2V and discharged at a voltage of 3.2V, and charged and discharged at a rate of 1C at room temperature. After 300 charge and discharge cycles, the battery was disassembled and observed for wrinkles and fractures on the interface and the current collector.
[0036] Example 2: Copper raw materials such as copper wire with a purity of ≥99.9%, copper plate with a purity of ≥99.9%, etc. are added to a copper dissolving tank in a ratio of 1:1 together with sulfuric acid and deionized water. Under the condition of high-temperature steam introduced by a screw fan, copper and sulfuric acid undergo an oxidation reaction to generate a copper sulfate electrolyte. After three-stage filtration through a diatomaceous earth filter, a security filter, and a precision filter, a pure copper sulfate electrolyte is obtained. Subsequently, hydrochloric acid and an organic composite electrolyte additive are added. The copper ion concentration in the copper sulfate aqueous solution is 90 g / L, and the sulfuric acid content is 105 g / L. The flow rate is 45 m 3 / h, the electrolyte with a temperature of 55℃ is transported to the foil machine, and the current density is 5500A / m 2 , produce 6μm copper foil, the raw foil is anti-oxidation treated, rolled, aged and slit to obtain the finished foil.
[0037] The hydrochloric acid is prepared into the electrolyte tank. - The concentration is 23 mg / L. The composite additive uses SPS (component A) with a concentration of 80 ppm; PEG with a molecular weight of 5000 (component B) with a concentration of 40 ppm; a mixture of 1,2-ethylene thiourea and 2-mercaptobenzothiazole in a ratio of 2:1 (component C) with a concentration of 50 ppm.
[0038] Three rolls of 800m copper foil were produced in batches. The raw foil samples were taken for testing. After baking at 150℃ for 10 minutes, the average tensile strength was measured to be 43.3kgf / mm 2 , weight deviation is 1.5% and average elongation is 6.7%.
[0039] The copper foil was used as the negative electrode current collector of the lithium secondary battery. By weight, 97 parts of commercially available graphite negative electrode were used as the negative electrode active material, mixed with 1 part of conductive carbon black, 1 part of styrene-butadiene rubber (SBR), 1 part of carboxymethyl cellulose (CMC) and 220 parts of deionized water to obtain a negative electrode slurry. A scraper was used to apply a 32 cm wide, 60 μm thick slurry on both sides of the copper foil, dried at 120°C, and heated at 1.0 t / cm 2 The negative electrode was pressed under pressure; and placed in an aluminum shell with the positive electrode, separator and electrolyte to make a 5PCS square lithium secondary battery. The battery was charged at a voltage of 4.2V and discharged at a voltage of 3.2V, and charged and discharged at a rate of 1C at room temperature. After 300 charge and discharge cycles, the battery was disassembled and observed for wrinkles and fractures on the interface and the current collector.
[0040] Example 3: Copper raw materials such as copper wire with a purity of ≥99.9%, copper plate with a purity of ≥99.9%, etc. are added to a copper dissolving tank in a ratio of 1:1 together with sulfuric acid and deionized water. Under the condition of high-temperature steam introduced by a screw fan, copper and sulfuric acid undergo oxidation reaction to generate copper sulfate electrolyte. After three-stage filtration through a diatomaceous earth filter, a security filter, and a precision filter, a pure copper sulfate electrolyte is obtained. Subsequently, hydrochloric acid and an organic composite electrolyte additive are added. The copper ion concentration in the copper sulfate aqueous solution is 90g / L, and the sulfuric acid content is 105g / L. The flow rate is 45m 3 / h, the electrolyte with a temperature of 55℃ is transported to the foil machine, and the current density is 5500A / m 2 , produce 6μm copper foil, the raw foil is anti-oxidation treated, rolled, aged and slit to obtain the finished foil.
[0041] The hydrochloric acid is prepared into the electrolyte tank. - The concentration is 25 mg / L. The composite additive uses SPS (component A) with a concentration of 80 ppm; PEG with a molecular weight of 5000 (component B) with a concentration of 45 ppm; a mixture of 1,2-ethylene thiourea and 2-mercaptobenzothiazole in a ratio of 2:1 (component C) with a concentration of 50 ppm.
[0042] Three rolls of 800m copper foil were produced in batches. The raw foil samples were taken for testing. After baking at 150℃ for 10 minutes, the average tensile strength was 41.0kgf / mm 2 , weight deviation is 2.1% and average elongation is 7.7%.
[0043] The copper foil was used as the negative electrode current collector of the lithium secondary battery. By weight, 97 parts of commercially available graphite negative electrode were used as the negative electrode active material, mixed with 1 part of conductive carbon black, 1 part of styrene-butadiene rubber (SBR), 1 part of carboxymethyl cellulose (CMC) and 220 parts of deionized water to obtain a negative electrode slurry. A scraper was used to apply a 32 cm wide, 60 μm thick slurry on both sides of the copper foil, dried at 120°C, and heated at 1.0 t / cm 2 The negative electrode was pressed under pressure; and placed in an aluminum shell with the positive electrode, separator and electrolyte to make a 5PCS square lithium secondary battery. The battery was charged at a voltage of 4.2V and discharged at a voltage of 3.2V, and charged and discharged at a rate of 1C at room temperature. After 300 charge and discharge cycles, the battery was disassembled and observed for wrinkles and fractures on the interface and the current collector.
[0044] Example 4: Copper raw materials such as copper wire with a purity of ≥99.9%, copper plate with a purity of ≥99.9%, etc. are added to a copper dissolving tank in a ratio of 1:1 together with sulfuric acid and deionized water. Under the condition of high-temperature steam introduced by a screw fan, copper and sulfuric acid undergo oxidation reaction to generate copper sulfate electrolyte. After three-stage filtration through a diatomaceous earth filter, a security filter, and a precision filter, a pure copper sulfate electrolyte is obtained. Subsequently, hydrochloric acid and an organic composite electrolyte additive are added. The copper ion concentration in the copper sulfate aqueous solution is 90g / L, and the sulfuric acid content is 105g / L. The flow rate is 45m 3 / h, the electrolyte with a temperature of 55℃ is transported to the foil machine, and the current density is 5500A / m 2 , produce 6μm copper foil, the raw foil is anti-oxidation treated, rolled, aged and slit to obtain the finished foil.
[0045] The hydrochloric acid is prepared into the electrolyte tank. - The concentration is 25 mg / L. The composite additive uses SPS (component A) with a concentration of 100 ppm; PEG with a molecular weight of 5000 (component B) with a concentration of 40 ppm; a mixture of 1,2-ethylene thiourea and 2-mercaptobenzothiazole in a ratio of 2:1 (component C) with a concentration of 50 ppm.
[0046] Three rolls of 800m copper foil were produced in batches. The raw foil samples were taken for testing. After baking at 150℃ for 10 minutes, the average tensile strength was measured to be 45.1kgf / mm 2 , weight deviation is 1.2% and average elongation is 6.1%.
[0047] The copper foil was used as the negative electrode current collector of the lithium secondary battery. By weight, 97 parts of commercially available graphite negative electrode were used as the negative electrode active material, mixed with 1 part of conductive carbon black, 1 part of styrene-butadiene rubber (SBR), 1 part of carboxymethyl cellulose (CMC) and 220 parts of deionized water to obtain a negative electrode slurry. A scraper was used to apply a 32 cm wide, 60 μm thick slurry on both sides of the copper foil, dried at 120°C, and heated at 1.0 t / cm 2 The negative electrode was pressed under pressure; and placed in an aluminum shell with the positive electrode, separator and electrolyte to make a 5PCS square lithium secondary battery. The battery was charged at a voltage of 4.2V and discharged at a voltage of 3.2V, and charged and discharged at a rate of 1C at room temperature. After 300 charge and discharge cycles, the battery was disassembled and observed for wrinkles and fractures on the interface and the current collector.
[0048] Example 5: Copper raw materials such as copper wire with a purity of ≥99.9%, copper plate with a purity of ≥99.9%, etc. are added to a copper dissolving tank in a ratio of 1:1 together with sulfuric acid and deionized water. Under the condition of high-temperature steam introduced by a screw fan, copper and sulfuric acid undergo oxidation reaction to generate copper sulfate electrolyte. After three-stage filtration through a diatomaceous earth filter, a security filter, and a precision filter, a pure copper sulfate electrolyte is obtained. Subsequently, hydrochloric acid and an organic composite electrolyte additive are added. The copper ion concentration in the copper sulfate aqueous solution is 90g / L, and the sulfuric acid content is 105g / L. The flow rate is 45m 3 / h, the electrolyte with a temperature of 55℃ is transported to the foil machine, and the current density is 5500A / m 2 , produce 6μm copper foil, the raw foil is anti-oxidation treated, rolled, aged and slit to obtain the finished foil.
[0049] The hydrochloric acid is prepared into the electrolyte tank. - The concentration is 25 mg / L. The composite additive uses SPS (component A) with a concentration of 100 ppm; PEG with a molecular weight of 5000 (component B) with a concentration of 45 ppm; a mixture of 1,2-ethylene thiourea and 2-mercaptobenzothiazole in a ratio of 2:1 (component C) with a concentration of 40 ppm.
[0050] Three rolls of 800m copper foil were produced in batches. The raw foil samples were taken for testing. After baking at 150℃ for 10 minutes, the average tensile strength was measured to be 43.2kgf / mm 2 , weight deviation is 1.7% and average elongation is 7.9%.
[0051] The copper foil was used as the negative electrode current collector of the lithium secondary battery. By weight, 96 parts of commercially available graphite negative electrode were used as the negative electrode active material, mixed with 1 part of conductive carbon black, 1.5 parts of styrene-butadiene rubber (SBR), 1.5 parts of carboxymethyl cellulose (CMC) and 220 parts of deionized water to obtain a negative electrode slurry. A scraper was used to apply a 32 cm wide, 60 μm thick slurry on both sides of the copper foil, dried at 120°C, and heated at 1.0 t / cm 2 The negative electrode was pressed under pressure; and placed in an aluminum shell with the positive electrode, separator and electrolyte to make a 5PCS square lithium secondary battery. The battery was charged at a voltage of 4.2V and discharged at a voltage of 3.2V, and charged and discharged at a rate of 1C at room temperature. After 300 charge and discharge cycles, the battery was disassembled and observed for wrinkles and fractures on the interface and the current collector.
[0052] Example 6: Copper raw materials such as copper wire with a purity of ≥99.9%, copper plate with a purity of ≥99.9%, etc. are added to a copper dissolving tank in a ratio of 1:1 together with sulfuric acid and deionized water. Under the condition of high-temperature steam introduced by a screw fan, copper and sulfuric acid undergo oxidation reaction to generate copper sulfate electrolyte. After three-stage filtration through a diatomaceous earth filter, a security filter, and a precision filter, a pure copper sulfate electrolyte is obtained. Subsequently, hydrochloric acid and an organic composite electrolyte additive are added. The copper ion concentration in the copper sulfate aqueous solution is 90g / L, and the sulfuric acid content is 105g / L. The flow rate is 45m 3 / h, the electrolyte with a temperature of 55℃ is transported to the foil machine, and the current density is 5500A / m 2 , produce 6μm copper foil, the raw foil is anti-oxidation treated, rolled, aged and slit to obtain the finished foil.
[0053] The hydrochloric acid is prepared into the electrolyte tank. - The concentration is 28 mg / L. The composite additive uses SPS (component A) with a concentration of 120 ppm; PEG with a molecular weight of 5000 (component B) with a concentration of 50 ppm; a mixture of 1,2-ethylene thiourea and 2-mercaptobenzothiazole in a ratio of 2:1 (component C) with a concentration of 40 ppm.
[0054] Three rolls of 800m copper foil were produced in batches. The raw foil samples were taken for testing. After baking at 150℃ for 10 minutes, the average tensile strength was measured to be 46.7kgf / mm 2 , weight deviation is 1.5% and average elongation is 8.8%.
[0055] The copper foil was used as the negative electrode current collector of the lithium secondary battery. By weight, 96 parts of commercially available graphite negative electrode were used as the negative electrode active material, mixed with 1 part of conductive carbon black, 1.5 parts of styrene-butadiene rubber (SBR), 1.5 parts of carboxymethyl cellulose (CMC) and 220 parts of deionized water to obtain a negative electrode slurry. A scraper was used to apply a 32 cm wide, 60 μm thick slurry on both sides of the copper foil, dried at 120°C, and heated at 1.0 t / cm 2 The negative electrode was pressed under pressure; and placed in an aluminum shell with the positive electrode, separator and electrolyte to make a 5PCS square lithium secondary battery. The battery was charged at a voltage of 4.2V and discharged at a voltage of 3.2V, and charged and discharged at a rate of 1C at room temperature. After 300 charge and discharge cycles, the battery was disassembled and observed for wrinkles and fractures on the interface and the current collector.
[0056] Example 7: Copper raw materials such as copper wire with a purity of ≥99.9%, copper plate with a purity of ≥99.9%, etc. are added to a copper dissolving tank in a ratio of 1:1 together with sulfuric acid and deionized water. Under the condition of high-temperature steam introduced by a screw fan, copper and sulfuric acid undergo an oxidation reaction to generate a copper sulfate electrolyte. After three-stage filtration through a diatomaceous earth filter, a security filter, and a precision filter, a pure copper sulfate electrolyte is obtained. Subsequently, hydrochloric acid and an organic composite electrolyte additive are added. The copper ion concentration in the copper sulfate aqueous solution is 90g / L, and the sulfuric acid content is 105g / L. The flow rate is 45m 3 / h, the electrolyte with a temperature of 55℃ is transported to the foil machine, and the current density is 5500A / m 2 , produce 6μm copper foil, the raw foil is anti-oxidation treated, rolled, aged and slit to obtain the finished foil.
[0057] The hydrochloric acid is prepared into the electrolyte tank. - The concentration is 28 mg / L. The composite additive uses SPS (component A) with a concentration of 120 ppm; PEG with a molecular weight of 5000 (component B) with a concentration of 50 ppm; a mixture of 1,2-ethylene thiourea and 2-mercaptobenzothiazole in a ratio of 2:1 (component C) with a concentration of 50 ppm.
[0058] Three rolls of 800m copper foil were produced in batches. The raw foil samples were taken for testing. After baking at 150℃ for 10 minutes, the average tensile strength was measured to be 43.9kgf / mm 2 , weight deviation is 1.9% and average elongation is 7.5%.
[0059] The copper foil was used as the negative electrode current collector of the lithium secondary battery. By weight, 97 parts of commercially available graphite negative electrode were used as the negative electrode active material, mixed with 1 part of conductive carbon black, 1 part of styrene-butadiene rubber (SBR), 1 part of carboxymethyl cellulose (CMC) and 220 parts of deionized water to obtain a negative electrode slurry. A scraper was used to apply a 32 cm wide, 60 μm thick slurry on both sides of the copper foil, dried at 120°C, and heated at 1.0 t / cm 2 The negative electrode was pressed under pressure; and placed in an aluminum shell with the positive electrode, separator and electrolyte to make a 5PCS square lithium secondary battery. The battery was charged at a voltage of 4.2V and discharged at a voltage of 3.2V, and charged and discharged at a rate of 1C at room temperature. After 300 charge and discharge cycles, the battery was disassembled and observed for wrinkles and fractures on the interface and the current collector.
[0060] Example 8: Copper raw materials such as copper wire with a purity of ≥99.9%, copper plate with a purity of ≥99.9%, etc. are added to a copper dissolving tank in a ratio of 1:1 together with sulfuric acid and deionized water. Under the condition of high-temperature steam introduced by a screw fan, copper and sulfuric acid undergo oxidation reaction to generate copper sulfate electrolyte. After three-stage filtration through a diatomaceous earth filter, a security filter, and a precision filter, a pure copper sulfate electrolyte is obtained. Subsequently, hydrochloric acid and an organic composite electrolyte additive are added. The copper ion concentration in the copper sulfate aqueous solution is 90g / L, and the sulfuric acid content is 105g / L. The flow rate is 45m 3 / h, the electrolyte with a temperature of 55℃ is transported to the foil machine, and the current density is 5500A / m 2 , produce 6μm copper foil, the raw foil is anti-oxidation treated, rolled, aged and slit to obtain the finished foil.
[0061] The hydrochloric acid is prepared into the electrolyte tank. - The concentration is 25 mg / L. The composite additive uses SPS (component A) with a concentration of 60 ppm; PEG with a molecular weight of 5000 (component B) with a concentration of 50 ppm; a mixture of 1,2-ethylene thiourea and 2-mercaptobenzothiazole in a ratio of 2:1 (component C) with a concentration of 40 ppm.
[0062] Three rolls of 800m copper foil were produced in batches. The raw foil samples were taken for testing. After baking at 150℃ for 10 minutes, the average tensile strength was measured to be 39.7kgf / mm 2 , weight deviation is 1.5% and average elongation is 6.1%.
[0063] The copper foil was used as the negative electrode current collector of the lithium secondary battery. By weight, 97 parts of commercially available graphite negative electrode were used as the negative electrode active material, mixed with 1 part of conductive carbon black, 1 part of styrene-butadiene rubber (SBR), 1 part of carboxymethyl cellulose (CMC) and 220 parts of deionized water to obtain a negative electrode slurry. A scraper was used to apply a 32 cm wide, 60 μm thick slurry on both sides of the copper foil, dried at 120°C, and heated at 1.0 t / cm 2 The negative electrode was pressed under pressure; and placed in an aluminum shell with the positive electrode, separator and electrolyte to make a 5PCS square lithium secondary battery. The battery was charged at a voltage of 4.2V and discharged at a voltage of 3.2V, and charged and discharged at a rate of 1C at room temperature. After 300 charge and discharge cycles, the battery was disassembled and observed for wrinkles and fractures on the interface and the current collector.
[0064] Comparative Example 1: Copper raw materials such as copper wire with a purity of ≥99.9%, copper plate with a purity of ≥99.9%, etc. are added to a copper dissolving tank together with sulfuric acid and deionized water in a ratio of 1:1. Under the condition of high-temperature steam introduced by a screw fan, copper and sulfuric acid undergo oxidation reaction to generate copper sulfate electrolyte. After three-stage filtration through a diatomaceous earth filter, a security filter, and a precision filter, a pure copper sulfate electrolyte is obtained. Subsequently, hydrochloric acid and an organic composite electrolyte additive are added. The copper ion concentration in the copper sulfate aqueous solution is 90g / L, and the sulfuric acid content is 105g / L. The flow rate is 45m 3 / h, the electrolyte with a temperature of 55℃ is transported to the foil machine, and the current density is 5500A / m 2 , produce 6μm copper foil, the raw foil is anti-oxidation treated, rolled, aged and slit to obtain the finished foil.
[0065] The hydrochloric acid is prepared into the electrolyte tank. - The concentration is 28 mg / L. The composite additive is a mixture of SPS and sodium methylene bisnaphthalene sulfonate in a ratio of 1:1 (component A), with a concentration of 100 ppm; PEG with a molecular weight of 5000 (component B), with a concentration of 40 ppm; and thiourea (component C), with a concentration of 50 ppm.
[0066] Three rolls of 800m copper foil were produced in batches. The raw foil samples were taken for testing. After baking at 150℃ for 10 minutes, the average tensile strength was measured to be 44.4kgf / mm 2 , weight deviation is 1.7% and average elongation is 8.4%.
[0067] The copper foil was used as the negative electrode current collector of the lithium secondary battery. By weight, 96 parts of commercially available graphite negative electrode were used as the negative electrode active material, mixed with 2 parts of conductive carbon black, 1 part of styrene-butadiene rubber (SBR), 1 part of carboxymethyl cellulose (CMC) and 220 parts of deionized water to obtain a negative electrode slurry. A scraper was used to apply a 32 cm wide, 60 μm thick slurry on both sides of the copper foil, dried at 120°C, and heated at 1.0 t / cm 2 The negative electrode was pressed under pressure; and placed in an aluminum shell with the positive electrode, separator and electrolyte to make a 5PCS square lithium secondary battery. The battery was charged at a voltage of 4.2V and discharged at a voltage of 3.2V, and charged and discharged at a rate of 1C at room temperature. After 300 charge and discharge cycles, the battery was disassembled and observed for wrinkles and fractures on the interface and the current collector.
[0068] Comparative Example 2: Copper raw materials such as copper wire with a purity of ≥99.9%, copper plate with a purity of ≥99.9%, etc. are added to a copper dissolving tank in a ratio of 1:1 together with sulfuric acid and deionized water. Under the condition of high-temperature steam introduced by a screw fan, copper and sulfuric acid undergo oxidation reaction to generate copper sulfate electrolyte. After three-stage filtration through a diatomaceous earth filter, a security filter, and a precision filter, a pure copper sulfate electrolyte is obtained. Subsequently, hydrochloric acid and an organic composite electrolyte additive are added. The copper ion concentration in the copper sulfate aqueous solution is 90g / L, and the sulfuric acid content is 105g / L. The flow rate is 45m 3 / h, the electrolyte with a temperature of 55℃ is transported to the foil machine, and the current density is 5500A / m 2 , produce 6μm copper foil, the raw foil is anti-oxidation treated, rolled, aged and slit to obtain the finished foil.
[0069] The hydrochloric acid is prepared into the electrolyte tank. - The concentration is 25 mg / L, and the composite additive adopts a mixture of SPS and sodium methylene bisnaphthalene sulfonate in a ratio of 1:1 (component A), with a concentration of 100 ppm; PEG with a molecular weight of 5000 (component B), with a concentration of 45 ppm; a mixture of 1,2-ethylene thiourea and 2-mercaptobenzothiazole in a ratio of 2:1 (component C), with a concentration of 40 ppm.
[0070] Three rolls of 800m copper foil were produced in batches. The raw foil samples were taken for testing. After baking at 150℃ for 10 minutes, the average tensile strength was 41.1kgf / mm 2 , weight deviation 2.0%, average elongation 9.3%.
[0071] The copper foil was used as the negative electrode current collector of the lithium secondary battery. By weight, 96 parts of commercially available graphite negative electrode were used as the negative electrode active material, mixed with 2 parts of conductive carbon black, 1 part of styrene-butadiene rubber (SBR), 1 part of carboxymethyl cellulose (CMC) and 220 parts of deionized water to obtain a negative electrode slurry. A scraper was used to apply a 32 cm wide, 60 μm thick slurry on both sides of the copper foil, dried at 120°C, and heated at 1.0 t / cm 2 The negative electrode was pressed under pressure; and placed in an aluminum shell with the positive electrode, separator and electrolyte to make a 5PCS square lithium secondary battery. The battery was charged at a voltage of 4.2V and discharged at a voltage of 3.2V, and charged and discharged at a rate of 1C at room temperature. After 300 charge and discharge cycles, the battery was disassembled and observed for wrinkles and fractures on the interface and the current collector.
[0072] Comparative Example 3: Copper raw materials such as copper wire with a purity of ≥99.9%, copper plate with a purity of ≥99.9%, etc. are added to a copper dissolving tank in a ratio of 1:1 together with sulfuric acid and deionized water. Under the condition of high-temperature steam introduced by a screw fan, copper and sulfuric acid undergo oxidation reaction to generate copper sulfate electrolyte. After three-stage filtration through a diatomaceous earth filter, a security filter, and a precision filter, a pure copper sulfate electrolyte is obtained. Subsequently, hydrochloric acid and an organic composite electrolyte additive are added. The copper ion concentration in the copper sulfate aqueous solution is 90g / L, and the sulfuric acid content is 105g / L. The flow rate is 45m 3 / h, the electrolyte with a temperature of 55℃ is transported to the foil machine, and the current density is 5500A / m 2 , produce 6μm copper foil, the raw foil is anti-oxidation treated, rolled, aged and slit to obtain the finished foil.
[0073] The hydrochloric acid is prepared into the electrolyte tank. - The concentration is 28 mg / L, and the composite additive adopts a mixture of SPS and sodium methylene bisnaphthalene sulfonate in a ratio of 1:1 (component A), with a concentration of 120 ppm; PEG with a molecular weight of 5000 (component B), with a concentration of 45 ppm; a mixture of 1,2-ethylene thiourea and 2-mercaptobenzothiazole in a ratio of 2:1 (component C), with a concentration of 40 ppm.
[0074] Three rolls of 800m copper foil were produced in batches. The raw foil samples were taken for testing. After baking at 150℃ for 10 minutes, the average tensile strength was measured to be 43.8kgf / mm 2 , weight deviation is 1.5% and average elongation is 6.4%.
[0075] The copper foil was used as the negative electrode current collector of the lithium secondary battery. By weight, 97 parts of commercially available graphite negative electrode as the negative electrode active material were mixed with 2 parts of conductive carbon black, 1 part of styrene-butadiene rubber (SBR), 1 part of carboxymethyl cellulose (CMC) and 220 parts of deionized water to obtain a negative electrode slurry. A scraper was used to apply a 32 cm wide, 60 μm thick slurry on both sides of the copper foil, dried at 120°C, and heated at 1.0 t / cm 2 The negative electrode was pressed under pressure; and placed in an aluminum shell with the positive electrode, separator and electrolyte to make a 5PCS square lithium secondary battery. The battery was charged at a voltage of 4.2V and discharged at a voltage of 3.2V, and charged and discharged at a rate of 1C at room temperature. After 300 charge and discharge cycles, the battery was disassembled and observed for wrinkles and fractures on the interface and the current collector.
[0076]
[0077]
[0078] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing copper foil with improved wrinkle problem, characterized in that: The following steps are involved: S1, preparing copper sulfate electrolyte; S2, adding hydrochloric acid and an organic composite electrolyte additive, wherein the organic composite electrolyte additive includes a brightener, a positioning agent, and a leveling agent; S3, electrolytically preparing raw foil, including electrolyzing raw foil under the conditions of a preset electrolyte temperature and a preset current density, wherein the preset electrolyte temperature is 40-60° C., and the preset current density is 3500 A / m 2 -6000 A / m 2 ; S4, performing anti-oxidation treatment on the surface of the electrolytic foil; S5, rolling, aging and slitting the raw foil into finished foil.
2. A method for preparing a copper foil with improved wrinkle problem according to claim 1, characterized in that: Preparation of copper sulfate electrolyte: First, copper raw materials such as copper wire with a purity of ≥99.9% and a diameter of 3-8mm, copper plate with a purity of ≥99.9% are added into a copper dissolving tank together with sulfuric acid and deionized water in a ratio of 1:1 or 1:
2. Under the condition of high-temperature steam passing through a screw fan, copper and sulfuric acid undergo an oxidation reaction to generate copper sulfate electrolyte. After three-stage filtration through a diatomaceous earth filter, a security filter, and a precision filter, a pure copper sulfate electrolyte is obtained.
3. The method for preparing a copper foil with improved wrinkle problem according to claim 2, characterized in that: The copper ion concentration in the copper sulfate aqueous solution is 70-90 g / L, and the sulfuric acid content is 100-120 g / L.
4. The method for preparing a copper foil with improved wrinkle problem according to claim 1, characterized in that: The hydrochloric acid is prepared by adding a hydrogen chloride solution with a content of 36%-38% into deionized water to prepare a hydrogen chloride aqueous solution with a concentration of 0.25%-0.5%.
5. The method for preparing a copper foil with improved wrinkle problem according to claim 1, characterized in that: The brightener includes sulfonic acid and its metal salt, including sodium polydisulfide propane sulfonate, sodium methylene dinaphthalene sulfonate, SH-110 sodium thiazoline disulfide propane sulfonate, or a mixture of two or more thereof. The brightener has both brightening and leveling effects, and inhibits defects generated during copper foil deposition. The added concentration range is 10-150ppm. The moving agent includes at least one of polyethylene glycol and polypropylene glycol, wherein the relative molecular weight of polyethylene glycol is 3000-6000, and the moving agent is a macromolecular additive, which blocks the diffusion of copper ions near the cathode, inhibits the electrodeposition of copper, and makes the copper foil more dispersed and flat. The added concentration range is 10-50ppm; The leveling agent includes at least one of unsaturated organic sulfides or nitrides, including one or a mixture of two or more of thiourea, 1,2-ethylenethiourea, 2-mercaptobenzimidazole, 2-mercaptobenzothiazole, and benzotriazole. The leveling agent is adsorbed on the protruding points on the surface of the copper foil through mutual interaction, promotes the electrodeposition of the concave parts of the copper foil, and plays a leveling role. The added concentration range is 5-50ppm.
6. The method for preparing a copper foil with improved wrinkle problem according to claim 4, characterized in that: The hydrochloric acid is added to the electrolyte to provide Cl - As a copper foil additive, the added concentration range is 18-40ppm, which plays a role of cathode depolarization in the electrodeposition process and promotes the deposition of copper. The preset electrolysis temperature of the electrolyte is 40-60°C, and the preset current density is 3500A / m 2 -6000 A / m 2 , the copper sulfate electrolyte flow rate is 30-50m3 / h.
7. The method for preparing a copper foil with improved wrinkle problem according to claim 1, characterized in that: The finished foil has a thickness of 4-10 μm, a weight deviation of ≤3%, and a tensile strength of 30-50 kgf / mm 2 , elongation ≥ 4%, and it has a bright surface and a matte surface, and the differences in Rz and Ra of the bright / matte surfaces are ≤ 0.5μm and 0.06μm respectively.
8. The method for preparing a copper foil with improved wrinkle problem according to claim 1, characterized in that: The finished foil has multiple oriented crystal planes, wherein the sum of the texture coefficients TC of the (111) plane and the (200) plane accounts for 30%-60% of the sum of the texture coefficients TC of the (111) plane, the (200) plane and the (220) plane, and can be used as copper foil for lithium secondary battery current collector.
9. A method for preparing a lithium secondary battery containing a copper foil with improved wrinkle problem as claimed in claim 1, characterized in that: The specific steps are as follows: Step 1: Preparation of negative electrode for lithium secondary battery: 90-98 parts by weight of commercially available graphite negative electrode as negative electrode active material, mixed with 0.5-2 parts of conductive carbon black, 0.5-1.5 parts of styrene-butadiene rubber (SBR), 0.5-1.5 parts of carboxymethyl cellulose (CMC) and 190-230 parts of deionized water to obtain negative electrode slurry, which is then coated on copper foil, dried, and rolled into a negative electrode sheet; Step 2: Place the positive electrode sheet, negative electrode sheet, separator and electrolyte in an aluminum shell to make a square lithium secondary battery.
10. The method for preparing a lithium secondary battery containing a copper foil with improved wrinkle problem according to claim 9, characterized in that: Use a scraper to apply 32cm wide, 60μm thick slurry on both sides of the copper foil, dry at 120℃, and 2 Pressing under pressure to form a negative electrode sheet; After the square lithium secondary battery was made, it was charged at a voltage of 4.2V and discharged at a voltage of 3.2V, with a charge and discharge rate of 1C at room temperature, and was cycled 300 times.
Citation Information
Patent Citations
Method for manufacturing ultrathin electrolytic copper foil
CN101476138A
Method for manufacturing two-sided optical ultrathin electrolytic copper foil with high elongation
CN101481810A
Method for producing 6-mu m ultra-thin electrolytic copper foil
CN102965699A
Preparation technology of negative electrode of lithium secondary battery
CN103700810A
Addition agent and process for producing 6-micron low-warping-degree electrolytic copper foil through addition agent
CN105002524A