Preparation method of reverse electrolytic copper foil as well as product and application of reverse electrolytic copper foil
By pickling, roughly curing, electroplating metal layer and silanization treatment of the electrolytic copper foil, the peel strength and heat resistance of the copper foil and the resin substrate are significantly improved by combining long chain and short chain silane coupling agent, and the peel strength and heat resistance of the copper foil and resin substrate are solved The shortcomings of PPO resin in high-temperature soldering and the bonding strength of copper foil are suitable for high-end copper clad plate manufacturing.
Patent Information
- Application Number
- CN202411149176.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-12
AI Technical Summary
High molecular weight functionalized polyphenylene ether (PPO) resins are difficult to withstand the challenges of high-temperature soldering in PCB processing, and their high melt viscosity limits the processing and forming ability. The bonding strength between untreated copper foil and semi-cured sheet is insufficient, affecting the product. Reliability; Traditional silane coupling agents have difficulties in electrical properties and heat resistance.
The silane coupling agent blend is prepared by a combination of long-chain silane coupling agent and short-chain silane coupling agent, and the electrolytic copper foil is pickled, cured, electroplating metal layer and silanization treatment is carried out, and the electroplating metal layer is passed through a specific electroplating metal layer. Process parameters and silanization treatment steps significantly improve the peel strength and heat resistance of the copper foil and the resin substrate.
The peel strength and heat resistance of the inverted electrolytic copper foil and PPO resin substrate are significantly improved, and are suitable for copper clad plate manufacturing for high-end electronic products, optimizing the balance between the surface roughness and electrical performance of the copper foil.
Smart Images

Figure BDA0005003120720000091 
Figure BDA0005003120720000101 
Figure BDA0005003120720000102
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of copper-clad laminates, and in particular relates to a method for preparing a reverse electrolytic copper foil, a product thereof and an application thereof. Background Art
[0002] With the rapid progress in the field of copper clad laminate (CCL) technology, the market trend has gradually shifted from traditional FR-4 products to high-end CCL products that pursue lower dielectric loss, accompanied by a profound change in the resin system, that is, from the classic epoxy resin system to a more functional non-epoxy system, especially the introduction of functionalized polyphenylene ether (PPO). However, as a thermoplastic resin, high molecular weight PPO has excellent performance, but it faces poor solvent resistance and is difficult to withstand the high temperature soldering challenge in PCB processing. In addition, its high melt viscosity limits the processing and molding capabilities, which directly limits its application in PCB insulating resin matrix.
[0003] To solve this problem, modifying PPO resin becomes the key path, aiming to convert it into thermosetting resin, thereby giving it good copper clad laminate processing performance and meeting the industry's demand for high-performance materials.
[0004] On the other hand, copper foil is one of the core raw materials for CCL manufacturing, and its performance directly affects the quality of the final product. At present, the insufficient bonding strength between copper foil and prepreg (PP) without special treatment has become a key factor restricting product reliability and leading to low peel strength, making it difficult to meet the stringent requirements of high-end electronic products.
[0005] From the perspective of fine processing of raw material copper foil, the strategies to improve the surface roughness (PS) of copper foil are subtle and diverse, aiming to balance the delicate relationship between physical bonding force and electrical performance. On the one hand, the high-roughness copper foil surface can significantly improve the physical bite force with the substrate. However, in high-frequency circuit applications, the "skin effect" is significant, and the current prefers to flow in the tiny tooth-like structure on the surface of the copper foil. Excessive surface roughness will increase power loss and insertion loss, affecting signal transmission efficiency.
[0006] On the other hand, silane coupling agents are introduced to coat the surface of copper foil, thereby enhancing the bonding between copper foil and resin. However, the development of traditional single silane coupling agents has difficulties including: 1) the silane chain is short and the molecular weight is small, which cannot meet the downstream requirements for bonding and heat resistance; 2) the silane molecular weight is large, and it is easy to self-polymerize and produce precipitation during hydrolysis, which is not easy to mass produce. Summary of the invention
[0007] In view of the above problems, the present invention discloses a method for preparing a reverse electrolytic copper foil. By modifying the surface of the electrolytic copper foil, the peel strength between the electrolytic copper foil and the resin substrate can be significantly improved, and the heat resistance of the electrolytic copper foil is also significantly improved; the reverse electrolytic copper foil prepared by this method is particularly suitable for PPO resin substrate.
[0008] To achieve the above purpose, the specific technical solution of the present invention is as follows:
[0009] A method for preparing reverse electrolytic copper foil comprises sequentially performing pickling treatment, rough curing treatment, electroplating a metal layer and silanization treatment on the raw foil, wherein the silanization treatment specifically comprises:
[0010] Adding a long-chain silane coupling agent and a short-chain silane coupling agent into acidic pure water, coating them on the treated surface of the copper foil after being fully hydrolyzed, and drying them to obtain a reverse electrolytic copper foil;
[0011] The long-chain silane coupling agent is selected from 3-acryloxypropyltrimethoxysilane;
[0012] The short-chain silane coupling agent is selected from one or more of vinyl trimethoxy silane and / or vinyl triethoxy silane;
[0013] The pH value of the pure water is 4 to 5;
[0014] The electroplated metal layers are sequentially electroplated metal nickel layers, electroplated metal zinc layers, electroplated metal chromium layers and electroplated nickel-chromium alloy layers; when electroplating the metal layers, the current density is 0.65-2.00A / dm 2 .
[0015] In the preparation method disclosed in the present invention, a silane coupling agent blend prepared by combining a specific long-chain silane coupling agent and a short-chain silane coupling agent is used to modify the electrolytic copper foil after pickling, rough curing and electroplating of the metal layer, which can significantly improve the peel strength between the electrolytic copper foil and the resin-based carrier, especially the PPO resin, and can also significantly improve the heat resistance of the electrolytic copper foil.
[0016] The experiment found that compared with the use of two silane coupling agents alone, the peel strength and heat resistance of the electrolytic copper foil prepared by using a combination of a specific long-chain silane coupling agent and a short-chain silane coupling agent have been significantly improved; if any one of the combination is replaced, the peel strength and heat resistance of the prepared electrolytic copper foil will be affected, and even lead to inferiority to the electrolytic copper foil prepared by a single silane coupling agent.
[0017] Preferably, the mass ratio of the long-chain silane coupling agent to the short-chain silane coupling agent is (1-3):1.
[0018] Further preferred:
[0019] The long-chain silane coupling agent is selected from 3-acryloxypropyltrimethoxysilane, and the short-chain silane coupling agent is selected from vinyltrimethoxysilane, and the mass ratio of the two is 3:1.
[0020] It was found through experiments that the electrolytic copper foil prepared by the above combination has the best peeling strength and heat resistance.
[0021] It was found in the experiment that during the silanization treatment, the appropriate acidity of pure water is also crucial for preparing electrolytic copper foil with high PS and high heat resistance. When only pure water is used without adjusting its pH value, the PS and heat resistance of the prepared electrolytic copper foil are significantly affected. Preferably, the pH value of the pure water is 4.
[0022] Preferably, the mass ratio of the total weight of the long-chain silane coupling agent and the short-chain silane coupling agent to pure water is 1:(100-500); more preferably 1:(200-450).
[0023] The experiment also found that the process parameters in the electroplating metal layer step before the silanization treatment step, especially the control of current density, also have a key influence on the heat resistance and PS of the final electrolytic copper foil.
[0024] Preferred:
[0025] When electroplating a metal nickel layer, the nickel ion concentration in the plating solution is 20-25 g / L, the boric acid concentration is 23-27 g / L, and the hypophosphite ion concentration is 8-12 g / L; the current density is 0.65-2.00 A / dm 2 , specifically, it can be 0.65, 0.66, 0.67, 0.68, 0.69, 0.70, 0.71, 0.72, 0.73, 0.74, 0.75, 0.80, 0.85, 0.89, 0.90, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0 or any value within the range;
[0026] When electroplating the metal zinc layer, the zinc ion concentration in the plating solution is 7-12 g / L, the boric acid concentration is 23-27 g / L; the current density is 0.65-2.00 A / dm 2 , specifically, it can be 0.65, 0.66, 0.67, 0.68, 0.69, 0.70, 0.71, 0.72, 0.73, 0.74, 0.75, 0.80, 0.85, 0.89, 0.90, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0 or any value within the range;
[0027] When electroplating the metal chromium layer, the chromium ion concentration in the plating solution is 2.5-5.0 g / L, the phosphate ion concentration is 1050-1250 mg / L; the current density is 0.65-2.00 A / dm 2 , specifically, it can be 0.65, 0.66, 0.67, 0.68, 0.69, 0.70, 0.71, 0.72, 0.73, 0.74, 0.75, 0.80, 0.85, 0.89, 0.90, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0 or any value within the range;
[0028] When electroplating the nickel-chromium alloy layer, the chromium ion concentration in the plating solution is 2.5-3.0 g / L, the nickel ion concentration is 1-3 g / L, the phosphate ion concentration is 1000-1100 mg / L, and the sulfate ion concentration is 2220-2400 mg / L; the current density is 0.65-2.00 A / dm 2 , specifically can be 0.65, 0.66, 0.67, 0.68, 0.69, 0.70, 0.71, 0.72, 0.73, 0.74, 0.75, 0.80, 0.85, 0.89, 0.90, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0 or any value within the range.
[0029] In the above electroplating steps, the plating solution temperature is controlled at 20-50°C.
[0030] Further preferred:
[0031] When electroplating the metal nickel layer, the current density is 0.85~1.50A / dm 2 ;
[0032] When electroplating the metal zinc layer, the current density is 0.85~1.50A / dm 2 ;
[0033] When electroplating the metal chromium layer, the current density is 0.85~1.50A / dm 2 ;
[0034] When electroplating the nickel-chromium alloy layer, the current density is 0.85~1.50A / dm 2 .
[0035] It has been found through experiments that the peel strength and heat resistance of the electrolytic copper foil prepared by electroplating the metal layer with the above further preferred current density and then performing a subsequent silanization treatment are better.
[0036] In the present invention:
[0037] The pickling treatment uses an acidic solution at a treatment temperature of 10 to 50°C;
[0038] The rough curing treatment includes a roughening treatment and a curing treatment;
[0039] In the roughening treatment, the copper ion concentration in the plating solution is 5-30 g / L, the sulfuric acid concentration is 50-200 g / L, the plating solution temperature is 10-40° C., and the roughening current density is 6-30 A / dm 2 ;
[0040] In the curing treatment, the copper ion concentration in the plating solution is 30-100 g / L, the sulfuric acid concentration is 40-180 g / L, the plating solution temperature is 10-40° C., and the curing current density is 6-30 A / dm 2 .
[0041] The present invention also discloses a reverse electrolytic copper foil prepared according to the above method. After hot pressing the reverse electrolytic copper foil with a PPO resin substrate, the reverse electrolytic copper foil is tested and found to have excellent peel strength and heat resistance, and can be used to prepare resin-based copper-clad laminates, especially PPO resin-based copper-clad laminates.
[0042] Compared with the prior art, the present invention has the following beneficial results:
[0043] The invention discloses a method for preparing a reverse electrolytic copper foil, which can significantly improve the peeling strength between the prepared reverse electrolytic copper foil and a resin substrate, especially a PPO resin substrate, and the heat resistance of the reverse electrolytic copper foil by using a silane coupling agent blend prepared with a special composition to modify the surface of the copper foil and coordinating the process parameters in the electroplating metal layer step before the silanization treatment step, especially the precise control of the current density. The method is expected to be widely used in the field of resin-based copper clad laminates, especially PPO resin-based copper clad laminates. DETAILED DESCRIPTION
[0044] The present invention is further described in detail below in conjunction with examples and comparative examples, but the embodiments of the present invention are not limited thereto.
[0045] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present invention were purchased through commercial channels.
[0046] Example 1
[0047] (1) Pickling treatment
[0048] The raw foil was pickled in a 15 wt % sulfuric acid aqueous solution at 25°C.
[0049] (2) Rough curing treatment
[0050] The raw foil after pickling is subjected to rough curing treatment, and the treatment process is roughening → curing;
[0051] The copper ion concentration in the plating solution used for the roughening treatment is 15g / L, the sulfuric acid concentration is 120g / L, the plating temperature is 35°C, and the current density of the roughening treatment is 25A / dm 2 ;
[0052] The copper ion concentration in the plating solution used for the curing treatment is 55g / L, the sulfuric acid concentration is 100g / L, the plating temperature is 40℃, and the current density of the curing treatment is 30A / dm 2 .
[0053] (3) Electroplated metal layer
[0054] The electroplated composite metal layer is a metal nickel layer, a metal zinc layer, a metal chromium layer and a nickel-chromium alloy layer in sequence.
[0055] Metal plating ①: The nickel ion concentration in the plating solution is 20g / L, the boric acid concentration is 23g / L, the hypophosphite ion is 8g / L, the pH is 3-4, and the current density is 0.89A / dm 2 ;
[0056] Metal plating ②: The zinc ion concentration in the plating solution is 7g / L, the boric acid concentration is 23g / L, the pH is 3-4, and the current density is 1.18A / dm 2 ;
[0057] Metal plating ③: The chromium ion concentration in the plating solution is 2.5g / L, the phosphate ion concentration is 1050mg / L, and the current density is 0.89A / dm 2 ;
[0058] Metal plating ④: The chromium ion concentration in the plating solution is 2.5g / L, the nickel ion concentration is 1g / L, the phosphate ion concentration is 1100mg / L, the sulfate ion concentration is 2400mg / L, the pH is 3-4, and the current density is 1.04A / dm 2 .
[0059] (4) Silanization treatment
[0060] Weigh 247g pure water, adjust pH to 4 with acetic acid; add 0.3g vinyltrimethoxysilane and 0.9g 3-acryloxypropyltrimethoxysilane, stir and hydrolyze at room temperature 27°C for 6h, and the stirring speed is 300r / min;
[0061] The obtained silane coupling agent blend is coated on the treated surface of the copper foil, and then dried at 100° C. to obtain a reverse electrolytic copper foil.
[0062] Example 2
[0063] The preparation process is basically the same as that in Example 1, except that in step (4):
[0064] The mass of 3-acryloxypropyltrimethoxysilane was replaced with 0.6 g.
[0065] Example 3
[0066] The preparation process is basically the same as that in Example 1, except that in step (4):
[0067] The mass of 3-acryloxypropyltrimethoxysilane was replaced with 0.3 g.
[0068] Example 4
[0069] The preparation process is basically the same as that in Example 1, except that in step (4):
[0070] Vinyltrimethoxysilane was replaced with an equal mass of vinyltriethoxysilane.
[0071] Example 5
[0072] The preparation process is basically the same as that in Example 1, except that in step (4):
[0073] Weigh 247 g of pure water and adjust the pH to 5 with acetic acid.
[0074] Example 6
[0075] The preparation process is basically the same as that in Example 1, except that in step (3):
[0076] The current density of metal plating layer ① (the composition of the plating solution remains unchanged) is changed to 0.68A / dm 2 ; The current density of metal plating layer ② (the composition of the plating solution remains unchanged) is changed to 0.74A / dm 2 ; The current density of metal plating layer ③ (the composition of the plating solution remains unchanged) is changed to 0.89A / dm 2 ; The current density of metal plating layer ④ (the composition of the plating solution remains unchanged) is changed to 0.90A / dm 2 .
[0077] Example 7
[0078] The preparation process is basically the same as that in Example 1, except that in step (3):
[0079] The current density of metal plating layer ① (the composition of the plating solution remains unchanged) is changed to 1.30A / dm 2 ; The current density of metal plating layer ② (the composition of the plating solution remains unchanged) is changed to 1.40A / dm 2 ; The current density of metal plating layer ③ (the composition of the plating solution remains unchanged) is changed to 1.98A / dm 2 ; The current density of metal plating layer ④ (the composition of the plating solution remains unchanged) is replaced by 1.88A / dm2 .
[0080] Comparative Example 1
[0081] The preparation process is basically the same as that in Example 1, except that in step (4):
[0082] A single silane coupling agent, vinyltrimethoxysilane, was added, with a mass of 1.2 g.
[0083] Comparative Example 2
[0084] The preparation process is basically the same as that in Example 1, except that in step (4):
[0085] A single silane coupling agent, 3-acryloxypropyltrimethoxysilane, was added, with a mass of 1.2 g.
[0086] Comparative Example 3
[0087] The preparation process is basically the same as that in Example 1, except that in step (4):
[0088] A single silane coupling agent, vinylbenzylaminoethylaminopropyltrimethoxysilane, was added, with a mass of 1.2 g.
[0089] Comparative Example 4
[0090] The preparation process is basically the same as that in Example 1, except that in step (4):
[0091] 3-Acryloxypropyltrimethoxysilane was replaced with an equal mass of vinylbenzylaminoethylaminopropyltrimethoxysilane.
[0092] Comparative Example 5
[0093] The preparation process is basically the same as that in Example 1, except that in step (4):
[0094] Weigh 247 g of pure water, pH = 7; add 0.3 g of vinyltrimethoxysilane and 0.9 g of 3-acryloxypropyltrimethoxysilane, and stir and hydrolyze at room temperature 27° C. for 6 h at a stirring speed of 300 r / min.
[0095] Comparative Example 6
[0096] The preparation process is basically the same as that in Example 1, except that in step (3):
[0097] The current density of metal plating layer ① (the composition of the plating solution remains unchanged) is changed to 0.59A / dm 2 ; The current density of metal plating layer ② (the composition of the plating solution remains unchanged) is changed to 0.74A / dm 2 ; The current density of metal plating layer ③ (the composition of the plating solution remains unchanged) is changed to 0.89A / dm2 ; The current density of metal plating layer ④ (the composition of the plating solution remains unchanged) is replaced by 0.89A / dm 2 .
[0098] Comparative Example 7
[0099] The preparation process is basically the same as that in Example 1, except that in step (3):
[0100] The current density of metal plating layer ① (the composition of the plating solution remains unchanged) is changed to 0.44A / dm 2 ; The current density of metal plating layer ② (the composition of the plating solution remains unchanged) is changed to 0.89A / dm 2 ; The current density of metal plating layer ③ (the composition of the plating solution remains unchanged) is changed to 0.89A / dm 2 ; The current density of metal plating layer ④ (the composition of the plating solution remains unchanged) is replaced by 0.89A / dm 2 .
[0101] Performance Testing:
[0102] The reverse electrolytic copper foil prepared in each embodiment and comparative example was subjected to high temperature pressing with a PPO substrate (stage one: 30°C, 7psi, 40min; stage two: 220°C, 15psi, 60min; stage two: 30°C, 15psi, 20min), and the products were evaluated for peel strength (refer to national standard GB / T29847-2013-7.3.3.2) and heat resistance (refer to national standard GB / T 29847-2013-7.3.3.3), and the specific values are listed in the following Tables 1 and 2, respectively.
[0103] Table 1
[0104]
[0105]
[0106] a: Blank sample is copper foil without silanization treatment.
[0107] b: The attenuation rate is the ratio of the difference between the normal PS and the PS after 20 minutes of tinning to the normal PS.
[0108] Table 2
[0109]
[0110] From the data in Table 1, it can be seen that the reverse electrolytic copper foil prepared in Example 1 has the highest peel strength with the PPO substrate, and the electrolytic copper foil also has the best heat resistance; and when the mass ratio of the long-chain silane coupling agent to the short-chain silane coupling agent in the silane coupling agent blend is changed (Examples 1 to 3), the PS and heat resistance will change accordingly. In the system disclosed in the present invention, the optimal mass ratio of the long-chain silane coupling agent to the short-chain silane coupling agent is 3:1.
[0111] When the types of long-chain silane coupling agent and short-chain silane coupling agent are changed, it is found that the PS and heat resistance of the prepared electrolytic copper foil will be significantly affected, especially the type of long-chain silane coupling agent. In the system disclosed in the present invention, vinyltrimethoxysilane and 3-acryloxypropyltrimethoxysilane are the best combination (Example 1). If the short-chain silane coupling agent is replaced by vinyltriethoxysilane (Example 4), the PS and heat resistance of the prepared electrolytic copper foil will decrease, but still higher than the electrolytic copper foil treated with a single silane coupling agent (Comparative Examples 1-2); but if the long-chain silane coupling agent is replaced by vinylbenzylaminoethylaminopropyltrimethoxysilane (Comparative Example 4), the PS and heat resistance of the prepared electrolytic copper foil are significantly reduced. Although the PS is slightly improved compared with the electrolytic copper foil prepared by using vinylbenzylaminoethylaminopropyltrimethoxysilane alone (Comparative Example 3), the heat resistance is even worse.
[0112] Comparative Examples 1, 5 and Comparative Example 5 also show that, during the silanization treatment, the appropriate acidity of pure water (pH = 4-5) is also crucial for preparing the electrolytic copper foil with high PS and high heat resistance.
[0113] Comparing the data in Table 2, it can be seen that even if the composition of the silane coupling agent blend in the silanization treatment step is optimized, the process parameter control in the previous electroplating metal layer step also has a key influence on the heat resistance and PS of the finally prepared electrolytic copper foil (Examples 1, 6, 7 and Comparative Examples 6, 7).
[0114] 2. The reverse electrolytic copper foil prepared in each embodiment and comparative example was subjected to high-temperature pressing with an epoxy resin substrate (manufacturer: Shengyi Technology, brand: S1000-2MB) (stage one: 190°C, 92.3psi, 20min; stage two: 190°C, 340psi, 100min; stage three: 40°C, 340.3psi, 40min); the peel strength and heat resistance of the samples were evaluated under the same test conditions as above. The specific values are listed in Table 3 below.
[0115] Table 3
[0116]
[0117] Comparing the data of the blank sample, Examples 1 to 4 and Comparative Examples 1 to 2 in Table 3, it can be seen that the reverse electrolytic copper foil prepared by the treatment with double-bond silane or compound silane has a very low compatibility with the epoxy substrate, the maximum improvement in peel strength is only 0.027N / mm, and the overall improvement in heat resistance is not obvious, and some even decrease. This is significantly different from the data in Table 1, indicating that the reverse electrolytic copper foil prepared by the method disclosed in the present invention has a higher degree of compatibility with the PPO substrate.
[0118] The above-mentioned embodiments are preferred embodiments, but the protection scope of the present invention is not limited thereto. A person skilled in the art can easily understand the spirit of the present invention based on the above-mentioned embodiments and make different extensions and changes. However, as long as they do not deviate from the spirit of the present invention, they are all within the protection scope of the present invention.
Claims
1. A method for preparing a reverse electrolytic copper foil, comprising sequentially performing pickling treatment, rough curing treatment, electroplating a metal layer and silanization treatment on the raw foil, It is characterized in that The silanization treatment specifically includes: Adding a long-chain silane coupling agent and a short-chain silane coupling agent into acidic pure water, coating them on the treated surface of the copper foil after being fully hydrolyzed, and drying them to obtain a reverse electrolytic copper foil; The long-chain silane coupling agent is selected from 3-acryloxypropyltrimethoxysilane; The short-chain silane coupling agent is selected from one or more of vinyl trimethoxy silane and / or vinyl triethoxy silane; The pH value of the pure water is 4 to 5; The electroplated metal layers are sequentially electroplated metal nickel layers, electroplated metal zinc layers, electroplated metal chromium layers and electroplated nickel-chromium alloy layers; when electroplating the metal layers, the current density is 0.65-2.00A / dm 2 .
2. The method for preparing the reverse electrolytic copper foil according to claim 1, It is characterized in that The mass ratio of the long-chain silane coupling agent to the short-chain silane coupling agent is (1-3):
1.
3. The method for preparing the reverse electrolytic copper foil according to claim 1, Features: The mass ratio of the total weight of the long-chain silane coupling agent and the short-chain silane coupling agent to pure water is 1:(100-500).
4. The method for preparing the reverse electrolytic copper foil according to claim 1, It is characterized in that The short-chain silane coupling agent is selected from vinyl triethoxy silane.
5. The method for preparing the reverse electrolytic copper foil according to claim 1, It is characterized in that The pH value of the pure water is 4.
6. The method for preparing the reverse electrolytic copper foil according to claim 1, Features: When electroplating a metal nickel layer, the nickel ion concentration in the plating solution is 20-25 g / L, the boric acid concentration is 23-27 g / L, and the hypophosphite ion concentration is 8-12 g / L; When electroplating a metal zinc layer, the zinc ion concentration in the plating solution is 7-12 g / L, and the boric acid concentration is 23-27 g / L; When electroplating a metal chromium layer, the chromium ion concentration in the plating solution is 2.5-5.0 g / L, and the phosphate ion concentration is 1050-1250 mg / L; When electroplating the nickel-chromium alloy layer, the chromium ion concentration in the plating solution is 2.5-3.0 g / L, the nickel ion concentration is 1-3 g / L, the phosphate ion concentration is 1000-1100 mg / L, and the sulfate ion concentration is 2220-2400 mg / L.
7. The method for preparing a reverse electrolytic copper foil according to claim 1, Features: The pickling treatment uses an acidic solution at a treatment temperature of 10 to 50°C; The rough curing treatment includes a roughening treatment and a curing treatment; In the roughening treatment, the copper ion concentration in the plating solution is 5-30 g / L, the sulfuric acid concentration is 50-200 g / L, the plating solution temperature is 10-40° C., and the roughening current density is 6-30 A / dm 2 ; In the curing treatment, the copper ion concentration in the plating solution is 30-100 g / L, the sulfuric acid concentration is 40-180 g / L, the plating solution temperature is 10-40° C., and the curing current density is 6-30 A / dm 2 .
8. A reverse electrolytic copper foil prepared by the method according to any one of claims 1 to 7.
9. A resin-based copper-clad laminate prepared using the reverse electrolytic copper foil according to claim 8.
10. The resin-based copper clad laminate according to claim 9, It is characterized in that The resin is selected from polyphenylene ether resin.