Aluminum alloy surface oxidation coloring method

By using oxidation solutions of trivalent manganese sulfate and glycerol phosphoric acid in the surface oxidation coloring method of aluminum alloy, the problems of unevenness and weather resistance during the tin salt coloring process are solved, and a more uniform and more stable surface chromatography effect of aluminum alloy is achieved. , expands the color gamut and improves surface hardness and weather resistance.

CN118932453APending Publication Date: 2024-11-12WUXI WKW AUTOMOTIVE PARTS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410827590.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing electrolytic coloring method of aluminum alloy oxide film, there is unevenness in the tin salt coloring process, poor weather resistance, and divalent tin is easily oxidized into tetravalent tin, which affects the stability and mechanical properties of the coloring.

Method used

A method of surface oxidation and coloring of aluminum alloys is adopted, including alkaline solution washing, acid solution activation and oxidation and coloring steps, using an oxidation solution containing trivalent manganese sulfate to stabilize divalent tin, combined with glycerol phosphoric acid to replace ethylenediaminetetraacetic acid, enhance Solution stability and deposition uniformity.

Benefits of technology

The color uniformity, weather resistance and surface hardness are improved, the color gamut is expanded, the production of tetravalent tin is reduced, and the color weather resistance and stability is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932453A_ABST
    Figure CN118932453A_ABST
Patent Text Reader

Abstract

The invention relates to an aluminum alloy surface oxidation coloring method which comprises the following steps: step 1, alkali liquor washing: firstly, washing an aluminum alloy plate clean, then putting the aluminum alloy plate in a solution containing a surfactant, and washing the aluminum alloy plate clean to obtain an alkali-treated aluminum alloy plate; 2, acid liquor activation is conducted, specifically, the alkali-treated aluminum alloy plate is placed in a solution containing mixed acid to be treated and washed clean, and an acid-activated aluminum alloy plate is obtained; and 3, oxidation coloring is conducted, specifically, the acid-activated aluminum alloy plate is subjected to oxidation coloring treatment, after oxidation coloring is completed, the aluminum alloy plate is washed clean with clear water, and the oxidation-colored aluminum alloy plate is obtained. The aluminum alloy surface oxidation coloring is uniform in coloring, good in weather resistance and higher in surface hardness. The invention is characterized in that: an oxidation solution containing a coloring agent is used, and trivalent manganese sulfate is especially added in the solution besides stannous sulfate, so that the stability and dispersity are enhanced, and the color system is expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of aluminum alloys, and in particular to a method for oxidation coloring of the surface of an aluminum alloy. Background Art

[0002] Aluminum alloy profiles are a commonly used building material. Before using aluminum alloy profiles, in order to improve the anti-corrosion performance of the profiles and have a certain color decorative effect, the profile surface must be treated. Aluminum alloy profile products are divided into electrolytic coloring, spraying organic coatings and other products according to the surface treatment method. Electrolytic coloring products are formed on the surface of aluminum alloy profiles through the principles of anodizing and electrolytic coloring. A dense oxide film is formed and a certain amount of non-ferrous metal ions are electrolytically reduced in the oxide film to present a certain color. The electrolytic coloring method can improve the decorative performance of aluminum profile products, and various tones can be freely obtained. It is widely used in the field of aluminum profile surface treatment.

[0003] The electrolytic coloring process of aluminum alloy oxide film has a fast coloring speed and has low requirements for the surface adsorption of the porous film layer. The electrolytic coloring process of oxide film is a process in which hydrogen ions and metal ions compete for discharge in an acidic metal salt solution. The oxide film to be colored is used as the cathode. After power is applied, the hydrogen ions in the solution pass through the barrier layer and obtain electrons at the contact interface between the aluminum base and the barrier layer to generate hydrogen. The metal ions are large in size, so they obtain electrons at the interface between the barrier layer and the electrolyte and exist in the form of metal particles or metal oxides or metal hydroxides.

[0004] The main electrolytic coloring methods for aluminum alloys include nickel salt coloring, tin salt coloring, and nickel-tin mixed salt coloring. For example, the coloring of tin salts can obtain different chromaticities from champagne to true black by changing the concentration of the main coloring salt (SnSO4). However, the disadvantage is that Sn 2+ The ions are very sensitive to light and air, and are easily oxidized into tetravalent tin compounds that have no coloring ability. This light gray flocculent mass is continuously precipitated with the increase of coloring time, and adheres to the current-intensive areas around the colored parts, thus affecting the coloring process; in addition, the current tin salt coloring process is prone to unevenness, and due to its poor weather resistance, it will gradually fade during use, and will also affect the mechanical properties of the aluminum alloy surface. Summary of the invention

[0005] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for oxidation coloring of aluminum alloy surface.

[0006] The purpose of the present invention is achieved by the following technical solutions:

[0007] A method for oxidizing and coloring the surface of an aluminum alloy comprises the following steps:

[0008] Step 1, lye washing:

[0009] First, the aluminum alloy plate is washed with clean water, then placed in a solution containing a surfactant, heated for a period of time, taken out, and then rinsed with clean water to obtain an alkali-treated aluminum alloy plate;

[0010] Step 2, acid activation:

[0011] The alkali-treated aluminum alloy plate is placed in a solution containing a mixed acid, heated for a period of time, and then rinsed with clean water to obtain an acid-activated aluminum alloy plate;

[0012] Step 3, oxidation coloring:

[0013] The acid-activated aluminum alloy plate is placed in an oxidizing solution containing a colorant for oxidation coloring. After the oxidation coloring is completed, it is rinsed with clean water to obtain an oxidation-colored aluminum alloy plate.

[0014] Preferably, in step 1, the solution components containing a surfactant include:

[0015] Sodium hydroxide 4-10g / L, surfactant 2-5g / L, the balance is water.

[0016] Preferably, the surfactant is an anionic surfactant, including sodium dodecylbenzene sulfonate, sodium hexadecylbenzene sulfonate or sodium octadecylbenzene sulfonate.

[0017] Preferably, in step 1, the temperature for the heating treatment is 40-50° C. and the time is 5-10 min.

[0018] Preferably, in step 2, the solution containing the mixed acid comprises:

[0019] 6-12g / L sulfuric acid, 12-24g / L phosphoric acid, the balance is water.

[0020] Preferably, in step 2, the temperature for the heating treatment is 45-55° C. and the time is 2-5 min.

[0021] Preferably, in step 3, the components of the oxidation solution containing the colorant include:

[0022] 10-20g / L sulfuric acid, 8-12g / L ethylenediaminetetraacetic acid, 2-6g / L glycerophosphoric acid, 10-15g / L stannous sulfate, 0.5-4g / L trivalent manganese sulfate, and the balance is water.

[0023] Preferably, in step 3, the parameters of oxidation coloring include:

[0024] The temperature is 15-20℃ and the current density is 2.7-4A / dm 2, the voltage is 25-50V, and the time is 1-10min.

[0025] The beneficial effects of the present invention are:

[0026] 1. The aluminum alloy surface oxidation coloring of the present invention is uniform in coloring, good in weather resistance, and has a higher surface hardness. The special feature of the present invention is that an oxidation solution containing a colorant is used, and in addition to stannous sulfate, trivalent manganese sulfate is added to the solution, which not only enhances stability and dispersibility, but also expands the color range due to the addition of manganese.

[0027] 2. In the current aluminum alloy oxidation coloring system, the most commonly used coloring metal is still divalent tin ion, which has a faster coloring speed, is relatively stable in coloring, and has a relatively small impact on environmental pollution. However, in the coloring process, due to the instability of divalent tin, it is easily oxidized to tetravalent tin. Tartaric acid or aminosulfonic acid is added in the prior art to prevent the oxidation of divalent tin and protect it. Although some effects have been achieved, the effect is not very ideal. The present invention introduces a trivalent manganese salt into the coloring oxidation solution. Since trivalent manganese has a strong reducibility, it will be gradually reduced to divalent manganese in the coloring oxidation solution, thereby better reducing the oxidation of divalent tin. At the same time, the divalent manganese ion obtained can participate in electrolytic reduction as a part of the coloring material.

[0028] 3. Although the traditionally used ethylenediaminetetraacetic acid (EDTA) has strong complexing compatibility, it lacks stability, especially after adding manganese, the overall stability performance is somewhat insufficient. Therefore, the present invention adds glycerophosphate to replace part of the EDTA, and it is found that the stability of the solution is well enhanced, which also has a greater impact on the subsequent deposition of ions, and the deposition coloring is more uniform.

[0029] 4. The addition of trivalent manganese sulfate not only greatly reduces the degree of oxidation of divalent tin and reduces the production of more tetravalent tin complexes, but also enhances the color of the deposit to a certain extent, expanding the color range of coloring, including champagne, bronze, coffee, bronze, dark brown and pure black. In addition, the inventors also found that the color weather resistance of the colored aluminum alloy plate is also enhanced. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The present invention is further described using the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the present invention. A person skilled in the art can obtain other drawings based on the following drawings without creative work.

[0031] Figure 1This is a comparison of photographs of the aluminum alloys after coloring treated with Example 1 of the present invention and Comparative Examples 1-3 (wherein a-Example 1, b-Comparative Example 1, c-Comparative Example 2, d-Comparative Example 3). DETAILED DESCRIPTION

[0032] In order to more clearly illustrate the present invention and have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.

[0033] In the current market, the most commonly used method for coloring aluminum alloys is tin salt coloring, but tin salt coloring is not very stable. During the coloring process, SnSO4 is easily oxidized to tetravalent tin. Tetravalent tin not only has poor coloring but also easily produces precipitation. Therefore, it is necessary to ensure that divalent tin is not oxidized during the coloring process. In addition, tin salts have the disadvantage of poor weather resistance, and gradually show signs of fading as the sun's exposure intensifies.

[0034] The sulfuric acid used in the present invention is concentrated sulfuric acid with a mass concentration of 98%.

[0035] The present invention will be further described below in conjunction with the following examples.

[0036] Example 1

[0037] A method for oxidizing and coloring the surface of an aluminum alloy comprises the following steps:

[0038] Step 1, lye washing:

[0039] First, the aluminum alloy plate is washed with clean water, then placed in a solution containing a surfactant, heated to 45°C, kept warm for 8 minutes, taken out, and then rinsed with clean water to obtain an alkali-treated aluminum alloy plate;

[0040] The surfactant-containing solution comprises 6 g / L of sodium hydroxide, 3 g / L of sodium dodecylbenzene sulfonate, and the balance of water.

[0041] Step 2, acid activation:

[0042] The alkali-treated aluminum alloy plate is placed in a solution containing a mixed acid, the temperature is raised to 50°C, and the temperature is kept for 3 minutes. After the acidification is completed, the plate is taken out and rinsed with clean water to obtain an acid-activated aluminum alloy plate;

[0043] The solution containing mixed acid includes: 10 g / L sulfuric acid, 20 g / L phosphoric acid, and the balance is water.

[0044] Step 3, oxidation coloring:

[0045] The acid activated aluminum alloy plate is placed in an oxidizing solution containing a colorant for oxidation coloring. The parameters of oxidation coloring include: temperature is 15-20°C, current density is 3.2A / dm 2 , the voltage is 45V, and the time is 6min. After the oxidation coloring is completed, rinse with clean water to obtain an oxidized colored aluminum alloy plate;

[0046] The components of the oxidizing solution containing the colorant include: 15g / L sulfuric acid, 10g / L ethylenediaminetetraacetic acid, 4g / L glycerophosphoric acid, 12g / L stannous sulfate, 2.5g / L trivalent manganese sulfate, and the balance is water.

[0047] Example 2

[0048] A method for oxidizing and coloring the surface of an aluminum alloy comprises the following steps:

[0049] Step 1, lye washing:

[0050] First, the aluminum alloy plate is washed with clean water, then placed in a solution containing a surfactant, heated to 40°C, kept warm for 6 minutes, taken out, and then rinsed with clean water to obtain an alkali-treated aluminum alloy plate;

[0051] The surfactant-containing solution comprises 8 g / L sodium hydroxide, 4 g / L sodium hexadecylbenzene sulfonate, and the balance is water.

[0052] Step 2, acid activation:

[0053] The alkali-treated aluminum alloy plate is placed in a solution containing a mixed acid, heated to 50°C, and kept warm for 4 minutes. After the acidification is completed, the plate is taken out and rinsed with clean water to obtain an acid-activated aluminum alloy plate.

[0054] The solution containing mixed acid includes: 8g / L sulfuric acid, 16g / L phosphoric acid, and the balance is water.

[0055] Step 3, oxidation coloring:

[0056] The acid activated aluminum alloy plate is placed in an oxidizing solution containing a colorant for oxidation coloring. The parameters of oxidation coloring include: temperature is 15-20°C, current density is 3.6A / dm 2 , the voltage is 35V, and the time is 5min. After the oxidation coloring is completed, rinse with clean water to obtain an oxidized colored aluminum alloy plate;

[0057] The components of the oxidizing solution containing the colorant include: 15g / L sulfuric acid, 10g / L ethylenediaminetetraacetic acid, 3g / L glycerophosphoric acid, 14g / L stannous sulfate, 2.8g / L trivalent manganese sulfate, and the balance is water.

[0058] Example 3

[0059] A method for oxidizing and coloring the surface of an aluminum alloy comprises the following steps:

[0060] Step 1, lye washing:

[0061] First, the aluminum alloy plate is washed with clean water, then placed in a solution containing a surfactant, heated to 40°C, kept warm for 5 minutes, taken out, and then rinsed with clean water to obtain an alkali-treated aluminum alloy plate;

[0062] The surfactant-containing solution comprises 4 g / L sodium hydroxide, 2 g / L sodium dodecylbenzene sulfonate, and the balance is water.

[0063] Step 2, acid activation:

[0064] The alkali-treated aluminum alloy plate is placed in a solution containing a mixed acid, heated to 45°C, and kept warm for 2 minutes. After the acidification is completed, the plate is taken out and rinsed with clean water to obtain an acid-activated aluminum alloy plate.

[0065] The solution containing mixed acid includes: 6g / L sulfuric acid, 12g / L phosphoric acid, and the balance is water.

[0066] Step 3, oxidation coloring:

[0067] The acid activated aluminum alloy plate is placed in an oxidizing solution containing a colorant for oxidation coloring. The parameters of oxidation coloring include: temperature is 15°C, current density is 2.7A / dm 2 , the voltage is 25V, and the time is 1min. After the oxidation coloring is completed, rinse with clean water to obtain an oxidized colored aluminum alloy plate;

[0068] The components of the oxidizing solution containing the colorant include: 10 g / L sulfuric acid, 8 g / L ethylenediaminetetraacetic acid, 2 g / L glycerophosphoric acid, 10 g / L stannous sulfate, 0.5 g / L trivalent manganese sulfate, and the balance is water.

[0069] Example 4

[0070] A method for oxidizing and coloring the surface of an aluminum alloy comprises the following steps:

[0071] Step 1, lye washing:

[0072] First, the aluminum alloy plate is washed with clean water, then placed in a solution containing a surfactant, heated to 50°C, kept warm for 10 minutes, taken out, and then rinsed with clean water to obtain an alkali-treated aluminum alloy plate;

[0073] The surfactant-containing solution comprises: 10 g / L sodium hydroxide, 5 g / L sodium octadecylbenzene sulfonate, and the balance is water.

[0074] Step 2, acid activation:

[0075] The alkali-treated aluminum alloy plate is placed in a solution containing a mixed acid, heated to 55°C, and kept warm for 5 minutes. After the acidification is completed, the plate is taken out and rinsed with clean water to obtain an acid-activated aluminum alloy plate.

[0076] The solution containing mixed acid includes: 12 g / L sulfuric acid, 24 g / L phosphoric acid, and the balance is water.

[0077] Step 3, oxidation coloring:

[0078] The acid activated aluminum alloy plate is placed in an oxidizing solution containing a colorant for oxidation coloring. The parameters of oxidation coloring include: temperature is 20°C, current density is 4A / dm 2 , the voltage is 50V, and the time is 10min. After the oxidation coloring is completed, rinse with clean water to obtain an oxidized colored aluminum alloy plate;

[0079] The components of the oxidizing solution containing the colorant include: 20g / L sulfuric acid, 12g / L ethylenediaminetetraacetic acid, 6g / L glycerophosphoric acid, 15g / L stannous sulfate, 4g / L trivalent manganese sulfate, and the balance is water.

[0080] Comparative Example 1

[0081] A method for oxidizing and coloring the surface of an aluminum alloy, which differs from Example 1 in that the oxidizing solution containing a colorant does not contain trivalent manganese sulfate and glycerophosphoric acid, and the rest is the same as Example 1. Specifically:

[0082] Step 1 and step 2 are the same as those in Example 1.

[0083] In step 3, the components of the oxidation solution containing the colorant include: 15 g / L sulfuric acid, 10 g / L ethylenediaminetetraacetic acid, 12 g / L stannous sulfate, and the balance is water.

[0084] Comparative Example 2

[0085] A method for oxidation coloring of aluminum alloy surface, which is different from the embodiment in that the oxidation solution containing the colorant does not contain trivalent manganese sulfate, and the rest is the same as the embodiment 1. Specifically:

[0086] Step 1 and step 2 are the same as those in Example 1.

[0087] In step 3, the components of the oxidation solution containing the colorant include: 15 g / L sulfuric acid, 10 g / L ethylenediaminetetraacetic acid, 4 g / L glycerophosphoric acid, 12 g / L stannous sulfate, and the balance is water.

[0088] Comparative Example 3

[0089] A method for oxidizing and coloring the surface of an aluminum alloy, which differs from Example 1 in that the oxidizing solution containing a colorant does not contain glycerophosphoric acid, and the rest is the same as Example 1. Specifically:

[0090] Step 1 and step 2 are the same as those in Example 1.

[0091] In step 3, the components of the oxidizing solution containing the colorant include: 15 g / L sulfuric acid, 10 g / L ethylenediaminetetraacetic acid, 12 g / L stannous sulfate, 2.5 g / L trivalent manganese sulfate, and the balance is water.

[0092] Experimental example

[0093] The aluminum alloy was processed according to the methods of Example 1 and Comparative Examples 1-3 respectively. The aluminum alloy plate was 2024 aluminum alloy. The colored aluminum alloy was subjected to corresponding tests.

[0094] Among them, the content of 2024 aluminum alloy is calculated by mass percentage, including: Si: 0.5%, Cu: 3.8%, Mg: 1.2%, Zn: 0.25%, Mn: 0.3%, Ti: 0.15%, Cr: 0.1%, Fe: 0.5%, and the balance is aluminum.

[0095] For the aluminum alloys treated in Example 1 and Comparative Examples 1-3, Figure 1 As shown, it can be seen that the coloring of Example 1 is more uniform.

[0096] The test results are shown in Table 1.

[0097] Table 1 Performance of aluminum alloy after coloring by different methods

[0098]

[0099] Xenon lamp irradiation is carried out in a LAB xenon lamp aging test chamber, and the wavelength range of the xenon lamp is 290 to 800 nm.

[0100] △E* ab Refers to the difference between two LAB color parameters, which is calculated after detection using a colorimeter. The calculation formula is ΔE* ab =[(△L*) 2 +(△a*) 2 +(△b*) 2 ] 1 / 2

[0101] According to the color difference △E* ab The numerical values ​​are classified into the following levels:

[0102] Level 1: 0<△E* ab ≤0.5: Very small or absent, an ideal match.

[0103] Level 2: 0.5<△E* ab ≤1: Slightly small, an acceptable match.

[0104] Level 3: 1<△E* ab ≤2: Slight to moderate, acceptable in some applications.

[0105] Level 4: 2<△E* ab ≤3.5: Moderate, acceptable in specific applications.

[0106] Level 5: 3.5<△E* ab ≤5: There is a gap, which is acceptable in specific applications.

[0107] Level 6: 5<△E* ab : Very large and unacceptable in most applications.

[0108] In summary, it can be seen from Table 1 that the method of Example 1 of the present invention not only has a higher surface hardness for aluminum alloy coloring, but also has a uniform color without floating dust. Even after aging for 1000 hours under xenon lamp irradiation, the gloss retention is still higher than 90%, and the color difference △E* is ab It can also reach level 1, which means that its coloring is uniform and its weather resistance is better.

[0109] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for oxidation coloring of aluminum alloy surface, characterized in that: The steps include: Step 1, lye washing: First, the aluminum alloy plate is washed with clean water, then placed in a solution containing a surfactant, heated for a period of time, taken out, and then rinsed with clean water to obtain an alkali-treated aluminum alloy plate; Step 2, acid activation: The alkali-treated aluminum alloy plate is placed in a solution containing a mixed acid, heated for a period of time, and then rinsed with clean water to obtain an acid-activated aluminum alloy plate; Step 3, oxidation coloring: The acid-activated aluminum alloy plate is placed in an oxidizing solution containing a colorant for oxidation coloring. After the oxidation coloring is completed, it is rinsed with clean water to obtain an oxidation-colored aluminum alloy plate.

2. The method for oxidizing and coloring the surface of an aluminum alloy according to claim 1, characterized in that: In the step 1, the solution components containing a surfactant include: Sodium hydroxide 4-10g / L, surfactant 2-5g / L, the balance is water.

3. The method for oxidizing and coloring the surface of an aluminum alloy according to claim 1, characterized in that: The surfactant is an anionic surfactant, including sodium dodecylbenzene sulfonate, sodium hexadecylbenzene sulfonate or sodium octadecylbenzene sulfonate.

4. The method for oxidizing and coloring the surface of an aluminum alloy according to claim 1, characterized in that: In the step 1, the temperature for the heating treatment is 40-50° C. and the time is 5-10 minutes.

5. The method for oxidizing and coloring the surface of an aluminum alloy according to claim 1, characterized in that: In step 2, the solution containing the mixed acid comprises: 6-12g / L sulfuric acid, 12-24g / L phosphoric acid, the balance is water.

6. The method for oxidizing and coloring the surface of an aluminum alloy according to claim 1, characterized in that: In step 2, the temperature for the heating treatment is 45-55° C. and the time is 2-5 minutes.

7. The method for oxidizing and coloring the surface of an aluminum alloy according to claim 1, characterized in that: In step 3, the components of the oxidation solution containing the colorant include: 10-20g / L sulfuric acid, 8-12g / L ethylenediaminetetraacetic acid, 2-6g / L glycerophosphoric acid, 10-15g / L stannous sulfate, 0.5-4g / L trivalent manganese sulfate, and the balance is water.

8. The method for oxidation coloring of aluminum alloy surface according to claim 1, characterized in that: In step 3, the parameters of oxidation coloring include: The temperature is 15-20℃ and the current density is 2.7-4A / dm 2 , the voltage is 25-50V, and the time is 1-10min.