Low-carbon steel hot-pressed thin plate and preparation process thereof

Through hot flattening, quenching, tempering and microarc oxidation treatment, combined with photocuring technology of modified nano alumina and water-based polyurethane composite emulsion, the bending, deformation and corrosion resistance of low-carbon steel sheets are solved, achieving high Flatness and excellent corrosion resistance, antibacterial and hydrophobic properties extend the service life.

CN118932457APending Publication Date: 2024-11-12HEBEI ZONGHENG GRP FENGNAN STEEL CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411066937.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During the preparation process, low-carbon steel thin plates are prone to bending, deformation and poor flatness, and are insufficient corrosion resistance and antibacterial properties, resulting in a shortened service life.

Method used

After hot flattening, quenching and tempering treatment, microarc oxidation treatment is carried out to form an alumina ceramic layer, and photocuring is performed with modified nanoalumina and photocurable aqueous polyurethane composite emulsion sealing liquid to form a sealing layer. Improve corrosion resistance and antibacterial properties.

Benefits of technology

By using modified nano alumina and aqueous polyurethane composite emulsion, a hot-pressed thin plate with excellent corrosion resistance, antibacterial properties and hydrophobicity is formed, which extends the service life and improves the flatness of the thin plate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004979625830000081
    Figure BDA0004979625830000081
  • Figure BDA0004979625830000091
    Figure BDA0004979625830000091
Patent Text Reader

Abstract

The invention relates to the technical field of steel plates, in particular to a low-carbon steel hot-pressed thin plate and a preparation process thereof.The preparation process comprises the steps that a low-carbon steel plate is subjected to hot-pressing flattening, quenching and annealing treatment, then micro-arc oxidation treatment is conducted, then hole sealing liquid prepared from modified nanometer aluminum oxide and photocurable waterborne polyurethane composite emulsion is coated, and photocuring treatment is conducted; wherein the modified nano aluminum oxide is formed by grafting nano aluminum oxide with 3-(methacryloyloxy) propyltrimethoxysilane and an organosilicon quaternary ammonium salt monomer; the preparation method comprises the following steps: by taking polyhydroxy bio-based polyol, 1, 4-butanediol and isophorone diisocyanate as raw materials, dimethylolpropionic acid as a hydrophilic chain extender and bisphenol A diglycidyl ether as a modifier, generating a bio-based polyurethane prepolymer under the action of catalysts stannous octoate and dibutyltin dilaurate; the photocurable waterborne polyurethane composite emulsion is prepared by taking pentaerythritol triacrylate as an end-capping reagent and introducing an organosilicon quaternary ammonium salt monomer as an antibacterial agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel plates, in particular to a low-carbon steel hot-pressed thin plate and a preparation process thereof. Background Art

[0002] With the advancement of science and technology and the increase in various industrial activities of mankind, steel, which has low cost, abundant resources, good mechanical properties and is suitable for large-scale production, has become the most used metal material by mankind. It is widely used in various fields of the national economy and is a very important strategic basic industrial product.

[0003] Low carbon steel refers to carbon steel with a carbon content of less than 0.25% in the steel category. For example, common grades such as Q195, Q235, and No. 20 are all low carbon steels. They have good weldability and processability and are inexpensive. However, when made into thin plates, they are prone to varying degrees of bending, deformation, and poor flatness. At the same time, when used as processed parts, they have problems such as poor corrosion resistance and antibacterial properties, which greatly shortens their service life. Summary of the invention

[0004] The object of the present invention is to provide a low-carbon steel hot-pressed sheet and a preparation process thereof, so as to solve the problems in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A preparation process of a low-carbon steel hot-pressed sheet comprises the following steps:

[0007] S1: hot pressing, quenching, and tempering the low-carbon steel plate in sequence, and then alkali washing, acid washing, water washing, and alcohol washing in sequence after cleaning, and drying to obtain a hot pressed thin plate;

[0008] S2: performing micro-arc oxidation treatment on the hot pressed thin plate to obtain a pre-treated thin plate having an alumina ceramic layer on the surface;

[0009] S3: preparing sealing liquid using modified nano-alumina and photocurable waterborne polyurethane composite emulsion;

[0010] S4: coating the sealing liquid on the surface of the pretreated thin plate, photocuring treatment, and drying to obtain a low-carbon steel hot-pressed thin plate.

[0011] Furthermore, the working conditions of the hot pressing treatment are: keeping warm at 480°C for 3 hours and keeping warm at 420°C for 2 hours.

[0012] Furthermore, the working conditions for the quenching treatment are: keeping at 800°C for 5 minutes and cooling with oil; the working conditions for the tempering treatment are: keeping at 400°C for 1 hour and cooling with the furnace.

[0013] Furthermore, the working conditions of micro-arc oxidation treatment are: forward voltage of 540V, pulse frequency of 1450Hz, forward duty cycle of 15%, negative voltage of 50V, positive-negative pulse ratio of 1:1, and power-on time of 30min; the composition of the electrolyte used for micro-arc oxidation is: deionized water as solvent, containing 4-6g / L sodium aluminate, 0.5-1.5g / L disodium hydrogen phosphate, 0.5-1.5g / L sodium carbonate, 0.5-1.5g / L sodium tetraborate, and 1-3mL / L glycerol.

[0014] Furthermore, the mass ratio of the modified nano-alumina and the photocurable aqueous polyurethane composite emulsion in the sealing liquid is 15-17%.

[0015] Further, the preparation of modified nano-alumina comprises the following steps:

[0016] (1) 1,8-naphthalene anhydride, N,N-dimethylethylenediamine and anhydrous ethanol are mixed, stirred for 3-4 hours, and subjected to rotary evaporation. The mixture is purified by silica gel column using a dichloromethane and methanol in a volume ratio of 10:1 as an eluent to obtain N-(2-(dimethylamino)ethyl)-naphthaleneimide;

[0017] (2) Under nitrogen protection, 3-chloropropyltrimethoxysilane, N-(2-(dimethylamino)ethyl)-naphthaleneimide and toluene are mixed, kept at 78-82° C. for 33-36 hours, and rotary evaporated to obtain an organosilicon quaternary ammonium salt monomer;

[0018] (3) 3-(isobutyleneoxy)propyltrimethoxysilane, organosilicon quaternary ammonium salt monomer and deionized water are mixed, the pH value is adjusted to 4, a mixed solution of nano-alumina and anhydrous ethanol is added, the temperature is raised to 58-62° C. and kept warm for 2-3 hours, and the mixture is washed, dried and ground to obtain modified nano-alumina.

[0019] Furthermore, the mass ratio of 3-(isomethacryloyloxy)propyltrimethoxysilane, organosilicon quaternary ammonium salt monomer, and nano-alumina is 2:1:3.

[0020] Further, the preparation of the photocurable aqueous polyurethane composite emulsion comprises the following steps:

[0021] 1) Under a nitrogen atmosphere, polyethylene glycol and epoxidized soybean oil are mixed, concentrated sulfuric acid is added, and the mixture is kept in an oil bath at 98-102° C. for 2-3 hours, sodium carbonate solution is added, the mixture is cooled, ethyl acetate is added, the mixture is washed with saturated sodium chloride water, dried with anhydrous magnesium sulfate, filtered, and rotary evaporated to obtain a polyhydroxy bio-based polyol;

[0022] 2) In a nitrogen atmosphere, polyhydroxy bio-based polyol, 1,4-butanediol and isophorone diisocyanate are mixed, heated to 68-72°C and kept warm for 1-2 hours, cooled to 42-45°C, acetone is added, dimethylol propionic acid and bisphenol A diglycidyl ether are added, heated to 48-52°C, stannous octoate and dibutyltin dilaurate are added and kept warm for 3-4 hours, pentaerythritol triacrylate is added and kept warm for 1-2 hours, a mixture of organosilicon quaternary ammonium salt monomer and deionized water is added, triethylamine is added and kept warm for 20-30 minutes, deionized water is added for emulsification for 1 hour, rotary evaporation is performed, a photoinitiator is added, and a photocurable waterborne polyurethane composite emulsion is obtained.

[0023] Furthermore, the mass ratio of the polyhydroxy bio-based polyol, 1,4-butanediol, isophorone diisocyanate, dimethylol propionic acid, bisphenol A diglycidyl ether, pentaerythritol triacrylate, and silicone quaternary ammonium salt monomer is 1.8:0.12:2:0.15:0.15:0.33:0.8.

[0024] Beneficial effects of the present invention:

[0025] The invention provides a low-carbon steel hot-pressed thin plate and a preparation process thereof. By controlling process parameters, the low-carbon steel plate is subjected to hot pressing, quenching and annealing treatments in sequence to obtain a high-flatness thin plate, which is then subjected to micro-arc oxidation treatment to in-situ grow an alumina ceramic layer on the surface of the steel plate, and then coated with a sealing liquid prepared by modified nano-alumina and a photocurable aqueous polyurethane composite emulsion, and subjected to photocuring treatment to obtain a hot-pressed thin plate having excellent corrosion resistance, antibacterial properties and hydrophobicity.

[0026] By controlling the process parameters of micro-arc oxidation, an alumina ceramic layer with uniform pores is formed on a low-carbon steel hot-pressed sheet, and then modified nano-alumina is introduced into the sealing liquid as a filler to fill the pores, thereby improving the bonding strength between the sealing liquid and the pretreated sheet and improving its corrosion resistance at the same time; wherein the modified nano-alumina is nano-alumina grafted with 3-(isobutyleneoxy)propyltrimethoxysilane and organosilicon quaternary ammonium salt monomers, and the introduction of 3-(isobutyleneoxy)propyltrimethoxysilane gives it an unsaturated and double bonds, so that it participates in the cross-linking of the film layer formed by the sealing liquid under the action of a photoinitiator, thereby making the modified nano-alumina firmly adhere to the sealing layer formed by the sealing liquid; the organic silicon quaternary ammonium salt monomer is 1,8-naphthalene anhydride and N,N-dimethylethylenediamine to synthesize N-(2-(dimethylamino)ethyl)-naphthalimide, which is then prepared by quaternization with 3-chloropropyltrimethoxysilane, wherein the naphthalimide is a naphthalene-containing hydrophobic group, which can more effectively improve the bactericidal property of the quaternary ammonium salt than the benzene-containing hydrophobic group, and improve its antibacterial and antifouling ability.

[0027] The invention adopts UV curing, an environmentally friendly curing technology with low energy consumption and fast curing speed, to form a protective sealing layer on the surface of a hot-pressed thin plate. In order to overcome the problems of oxygen inhibition and uneven crosslinking that are easily generated in the existing UV curing process, the invention adopts polyhydroxy bio-based polyols generated by ring-opening of cheap biomaterial epoxidized soybean oil with polyethylene glycol as polyols, 1,4-butanediol and isophorone diisocyanate as raw materials, dimethylol propionic acid as a hydrophilic chain extender, bisphenol A diglycidyl ether as a modifier, and generates bio-based polyurethane prepolymers under the action of catalysts such as stannous octoate and dibutyltin dilaurate. Pentaerythritol triacrylate is used as a capping agent, and a silicone quaternary ammonium salt monomer is introduced as an antibacterial agent. Deionized water is added for emulsification, and the prepolymer is mixed with a photoinitiator to prepare a photocurable waterborne polyurethane composite emulsion, and a complex crosslinking network is constructed with modified nano-alumina, thereby greatly improving the corrosion resistance, antibacterial property and hydrophobicity of the hot-pressed thin plate and extending the service life of the hot-pressed thin plate. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] It should be noted that if the embodiments of the present invention involve directional indications such as up, down, left, right, front, and back, the directional indication is only used to explain a specific posture such as the relative position relationship between the components, the movement status, etc. If the specific posture changes, the directional indication will also change accordingly. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the protection scope required by the present invention.

[0030] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.

[0031] Embodiment 1: A process for preparing a low carbon steel hot pressed sheet, comprising the following steps:

[0032] S1: hot pressing, quenching, and tempering the low-carbon steel plate in sequence, and then alkali washing, acid washing, water washing, and alcohol washing in sequence after cleaning, and drying to obtain a hot pressed thin plate;

[0033] The working conditions of hot pressing treatment are: 3 h at 480 °C and 2 h at 420 °C;

[0034] The working conditions for quenching treatment are: keeping at 800℃ for 5min and oil cooling; the working conditions for tempering treatment are: keeping at 400℃ for 1h and cooling with the furnace;

[0035] S2: performing micro-arc oxidation treatment on the hot pressed thin plate to obtain a pre-treated thin plate having an alumina ceramic layer on the surface;

[0036] The working conditions of micro-arc oxidation treatment are: forward voltage of 540V, pulse frequency of 1450Hz, 15% forward duty cycle, negative voltage of 50V, positive-negative pulse ratio of 1:1, and power-on time of 30min; the composition of the electrolyte used for micro-arc oxidation is: deionized water as solvent, containing 5g / L sodium aluminate, 1g / L disodium hydrogen phosphate, 1g / L sodium carbonate, 1g / L sodium tetraborate, and 2mL / L glycerol;

[0037] S3: preparing sealing liquid using modified nano-alumina and photocurable waterborne polyurethane composite emulsion;

[0038] The mass ratio of modified nano-alumina and photocurable waterborne polyurethane composite emulsion in the sealing liquid is 15%;

[0039] The preparation of modified nano-alumina includes the following steps:

[0040] (1) 0.69 g of 1,8-naphthalene anhydride, 1.03 g of N,N-dimethylethylenediamine, and 50 mL of anhydrous ethanol were mixed, stirred for 3 h, and subjected to rotary evaporation. The mixture was purified by silica gel column using a dichloromethane and methanol in a volume ratio of 10:1 as an eluent to obtain N-(2-(dimethylamino)ethyl)-naphthaleneimide;

[0041] (2) Under nitrogen protection, 2.08 g of 3-chloropropyltrimethoxysilane, 2.4 g of N-(2-(dimethylamino)ethyl)-naphthaleneimide, and 15 mL of toluene were mixed, kept at 78° C. for 36 h, and rotary evaporated to obtain an organosilicon quaternary ammonium salt monomer;

[0042] (3) 2 g of 3-(isobutyleneoxy)propyltrimethoxysilane, 1 g of organosilicon quaternary ammonium salt monomer, and 20 mL of deionized water were mixed, the pH was adjusted to 4, 3 g of nano-alumina and 15 mL of anhydrous ethanol were added, the temperature was raised to 58° C. and kept warm for 3 h, washed, dried, and ground to obtain modified nano-alumina;

[0043] The preparation of the photocurable aqueous polyurethane composite emulsion comprises the following steps:

[0044] 1) Under nitrogen atmosphere, 1.66 mmol polyethylene glycol and 1 mmol epoxidized soybean oil were mixed, 10 μL concentrated sulfuric acid was added, and the mixture was kept in an oil bath at 98°C for 3 h, 20 μL sodium carbonate solution was added, the mixture was cooled, 40 mL ethyl acetate was added, the mixture was washed with saturated sodium chloride water, dried with anhydrous magnesium sulfate and filtered, and rotary evaporated to obtain polyhydroxy bio-based polyols;

[0045] 2) Under a nitrogen atmosphere, 1.8 g of polyhydroxy bio-based polyol, 0.12 g of 1,4-butanediol, and 2 g of isophorone diisocyanate were mixed, heated to 68° C. and kept warm for 2 h, cooled to 42° C., 5 mL of acetone was added, 0.15 g of dihydroxymethylpropionic acid and 0.15 g of bisphenol A diglycidyl ether were added, heated to 48° C., 0.1 g of stannous octoate and 0.1 g of dibutyltin dilaurate were added and kept warm for 3 h, 0.33 g of pentaerythritol triacrylate was added and kept warm for 1 h, 0.8 g of organosilicon quaternary ammonium salt monomer and 5 mL of deionized water were added, 0.1 g of triethylamine was added and kept warm for 20 min, deionized water was added for emulsification for 1 h, rotary evaporated, 0.08 g of photoinitiator was added, and a photocurable aqueous polyurethane composite emulsion with a solid content of 35% was obtained;

[0046] S4: coating the sealing liquid on the surface of the pretreated thin plate, photocuring treatment, and drying to obtain a low-carbon steel hot-pressed thin plate.

[0047] Embodiment 2: A process for preparing a low carbon steel hot pressed sheet, comprising the following steps:

[0048] S1: hot pressing, quenching and tempering the low carbon steel plate in sequence, and then alkali washing, acid washing, water washing and alcohol washing in sequence after cleaning, and drying to obtain a hot pressed thin plate;

[0049] The working conditions of hot pressing treatment are: 3 h at 480 °C and 2 h at 420 °C;

[0050] The working conditions for quenching treatment are: keeping at 800℃ for 5min and oil cooling; the working conditions for tempering treatment are: keeping at 400℃ for 1h and cooling with the furnace;

[0051] S2: performing micro-arc oxidation treatment on the hot pressed thin plate to obtain a pre-treated thin plate having an alumina ceramic layer on the surface;

[0052] The working conditions of micro-arc oxidation treatment are: forward voltage of 540V, pulse frequency of 1450Hz, 15% forward duty cycle, negative voltage of 50V, positive-negative pulse ratio of 1:1, and power-on time of 30min; the composition of the electrolyte used for micro-arc oxidation is: deionized water as solvent, containing 5g / L sodium aluminate, 1g / L disodium hydrogen phosphate, 1g / L sodium carbonate, 1g / L sodium tetraborate, and 2mL / L glycerol;

[0053] S3: preparing sealing liquid using modified nano-alumina and photocurable waterborne polyurethane composite emulsion;

[0054] The mass ratio of modified nano-alumina and photocurable waterborne polyurethane composite emulsion in the sealing liquid is 16%;

[0055] The preparation of modified nano-alumina includes the following steps:

[0056] (1) 0.69 g of 1,8-naphthalene anhydride, 1.03 g of N,N-dimethylethylenediamine, and 50 mL of anhydrous ethanol were mixed, stirred for 3-4 h, and evaporated by rotary evaporation. The eluent was dichloromethane and methanol in a volume ratio of 10:1, and the silica gel column was used for purification to obtain N-(2-(dimethylamino)ethyl)-naphthaleneimide;

[0057] (2) Under nitrogen protection, 2.08 g of 3-chloropropyltrimethoxysilane, 2.4 g of N-(2-(dimethylamino)ethyl)-naphthaleneimide, and 15 mL of toluene were mixed, kept at 80° C. for 34 h, and rotary evaporated to obtain an organosilicon quaternary ammonium salt monomer;

[0058] (3) 2 g of 3-(isobutyleneoxy)propyltrimethoxysilane, 1 g of organosilicon quaternary ammonium salt monomer, and 20 mL of deionized water were mixed, the pH was adjusted to 4, 3 g of nano-alumina and 15 mL of anhydrous ethanol were added, the temperature was raised to 60° C. and kept warm for 2.5 h, washed, dried, and ground to obtain modified nano-alumina;

[0059] The preparation of the photocurable aqueous polyurethane composite emulsion comprises the following steps:

[0060] 1) Under a nitrogen atmosphere, 1.66 mmol of polyethylene glycol and 1 mmol of epoxidized soybean oil were mixed, 10 μL of concentrated sulfuric acid was added, and the mixture was kept in an oil bath at 100° C. for 2.5 h, 20 μL of sodium carbonate solution was added, the mixture was cooled, 40 mL of ethyl acetate was added, the mixture was washed with saturated sodium chloride water, dried with anhydrous magnesium sulfate and filtered, and rotary evaporated to obtain a polyhydroxy bio-based polyol;

[0061] 2) Under a nitrogen atmosphere, 1.8 g of polyhydroxy bio-based polyol, 0.12 g of 1,4-butanediol, and 2 g of isophorone diisocyanate were mixed, heated to 70°C and kept warm for 1.5 h, cooled to 43°C, 5 mL of acetone was added, 0.15 g of dihydroxymethylpropionic acid and 0.15 g of bisphenol A diglycidyl ether were added, heated to 50°C, 0.1 g of stannous octoate and 0.1 g of dibutyltin dilaurate were added and kept warm for 3.5 h, 0.33 g of pentaerythritol triacrylate was added and kept warm for 1.5 h, 0.8 g of organosilicon quaternary ammonium salt monomer and 5 mL of deionized water were added, 0.1 g of triethylamine was added and kept warm for 25 min, deionized water was added for emulsification for 1 h, rotary evaporated, 0.08 g of photoinitiator was added, and a photocurable aqueous polyurethane composite emulsion with a solid content of 35% was obtained;

[0062] S4: coating the sealing liquid on the surface of the pretreated thin plate, photocuring treatment, and drying to obtain a low-carbon steel hot-pressed thin plate.

[0063] Embodiment 3: A process for preparing a low carbon steel hot pressed sheet, comprising the following steps:

[0064] S1: hot pressing, quenching, and tempering the low-carbon steel plate in sequence, and then alkali washing, acid washing, water washing, and alcohol washing in sequence after cleaning, and drying to obtain a hot pressed thin plate;

[0065] The working conditions of hot pressing treatment are: 3 h at 480 °C and 2 h at 420 °C;

[0066] The working conditions for quenching treatment are: keeping at 800℃ for 5min and oil cooling; the working conditions for tempering treatment are: keeping at 400℃ for 1h and cooling with the furnace;

[0067] S2: performing micro-arc oxidation treatment on the hot pressed thin plate to obtain a pre-treated thin plate having an alumina ceramic layer on the surface;

[0068] The working conditions of micro-arc oxidation treatment are: forward voltage of 540V, pulse frequency of 1450Hz, 15% forward duty cycle, negative voltage of 50V, positive-negative pulse ratio of 1:1, and power-on time of 30min; the composition of the electrolyte used for micro-arc oxidation is: deionized water as solvent, containing 5g / L sodium aluminate, 1g / L disodium hydrogen phosphate, 1g / L sodium carbonate, 1g / L sodium tetraborate, and 2mL / L glycerol;

[0069] S3: preparing sealing liquid using modified nano-alumina and photocurable waterborne polyurethane composite emulsion;

[0070] The mass ratio of modified nano-alumina and photocurable waterborne polyurethane composite emulsion in the sealing liquid is 17%;

[0071] The preparation of modified nano-alumina includes the following steps:

[0072] (1) 0.69 g of 1,8-naphthalene anhydride, 1.03 g of N,N-dimethylethylenediamine, and 50 mL of anhydrous ethanol were mixed, stirred for 4 h, and subjected to rotary evaporation. The mixture was purified by silica gel column using a dichloromethane and methanol in a volume ratio of 10:1 as an eluent to obtain N-(2-(dimethylamino)ethyl)-naphthaleneimide;

[0073] (2) Under nitrogen protection, 2.08 g of 3-chloropropyltrimethoxysilane, 2.4 g of N-(2-(dimethylamino)ethyl)-naphthalimide, and 15 mL of toluene were mixed, kept at 82° C. for 33 h, and rotary evaporated to obtain an organosilicon quaternary ammonium salt monomer;

[0074] (3) 2 g of 3-(isobutyleneoxy)propyltrimethoxysilane, 1 g of organosilicon quaternary ammonium salt monomer, and 20 mL of deionized water were mixed, the pH was adjusted to 4, 3 g of nano-alumina and 15 mL of anhydrous ethanol were added, the temperature was raised to 62° C. and kept warm for 2 h, washed, dried, and ground to obtain modified nano-alumina;

[0075] The preparation of the photocurable aqueous polyurethane composite emulsion comprises the following steps:

[0076] 1) Under a nitrogen atmosphere, 1.66 mmol of polyethylene glycol and 1 mmol of epoxidized soybean oil were mixed, 10 μL of concentrated sulfuric acid was added, and the mixture was kept in an oil bath at 102° C. for 2 h, 20 μL of sodium carbonate solution was added, the mixture was cooled, 40 mL of ethyl acetate was added, the mixture was washed with saturated sodium chloride water, dried with anhydrous magnesium sulfate, filtered, and rotary evaporated to obtain a polyhydroxy bio-based polyol;

[0077] 2) Under a nitrogen atmosphere, 1.8 g of polyhydroxy bio-based polyol, 0.12 g of 1,4-butanediol, and 2 g of isophorone diisocyanate were mixed, heated to 72° C. and kept warm for 1 h, cooled to 45° C., 5 mL of acetone were added, 0.15 g of dihydroxymethylpropionic acid and 0.15 g of bisphenol A diglycidyl ether were added, heated to 52° C., 0.1 g of stannous octoate and 0.1 g of dibutyltin dilaurate were added and kept warm for 4 h, 0.33 g of pentaerythritol triacrylate was added and kept warm for 2 h, 0.8 g of organosilicon quaternary ammonium salt monomer and a mixture of 5 mL of deionized water were added, 0.1 g of triethylamine was added and kept warm for 30 min, deionized water was added for emulsification for 1 h, rotary evaporated, 0.03 g of photoinitiator was added, and a photocurable aqueous polyurethane composite emulsion with a solid content of 35% was obtained;

[0078] S4: coating the sealing liquid on the surface of the pretreated thin plate, photocuring treatment, and drying to obtain a low-carbon steel hot-pressed thin plate.

[0079] Comparative Example 1: Taking Example 3 as the control group, nano alumina was used to replace the modified nano alumina, and the other processes were normal.

[0080] Comparative Example 2: Taking Example 3 as the control group, the photocurable aqueous polyurethane composite emulsion was replaced by acrylic modified silicone resin (001: Langfang Wanteng Anticorrosion Materials Co., Ltd.), and the other processes were normal.

[0081] Comparative Example 3: Example 3 was used as a control group, in which no organosilicon quaternary ammonium salt monomer was prepared, and other processes were normal.

[0082] In the embodiment and the comparative example, the sealing liquid is coated on the surface of the pretreated thin plate at a depth of 15 μm; the working conditions of the light curing treatment are: irradiation with ultraviolet light of a wavelength of 365 nm for 2 minutes.

[0083] Sources of raw materials used (for demonstration purposes only):

[0084] Low carbon steel plate (thickness 0.6 mm): in terms of mass percentage, the composition is: carbon 0.18%, silicon 0.1%, manganese 0.81%, phosphorus 0.02%, sulfur 0.031%, boron 0.001, and the balance is iron; photoinitiator 2959 (5465): Hubei Zhenbo Chemical Co., Ltd.; 1,8-naphthalene anhydride 81-84-5: Hubei Kewode Chemical Co., Ltd.; glycerol G116203, N,N-dimethylethylenediamine D105347, 3-chloropropyltrimethoxysilane C106514, 3-(isobutyleneoxy)propyltrimethoxysilane S111153, nano-alumina A102091, polyethylene glycol P1 03718, epoxidized soybean oil E107074, 1,4-butanediol B110391, isophorone diisocyanate I109582, dimethylolpropionic acid B104539, bisphenol A diglycidyl ether B131786, stannous octoate T100108, dibutyltin dilaurate D100274, pentaerythritol triacrylate P192936, triethylamine T103285: Aladdin reagent; sodium aluminate, disodium hydrogen phosphate, sodium carbonate, sodium tetraborate, acetone, anhydrous ethanol, dichloromethane, methanol, toluene, concentrated sulfuric acid, sodium carbonate, ethyl acetate, sodium chloride, anhydrous magnesium sulfate, analytical grade: Sinopharm Group reagent.

[0085] Performance test: Testing the thin plates prepared in the embodiments and comparative examples;

[0086] Hydrophobicity: characterized by water contact angle, tested by measuring instrument, using 4μL deionized water droplets; Antibacterial property: Gram-positive bacteria Staphylococcus aureus was selected as the experimental bacteria, and the coating method was used for testing; Corrosion resistance: salt spray test was carried out with reference to GB / T1771-2007, cut into 150mm long and 100mm wide plates, put into a salt spray box, the temperature was 37℃, the sodium chloride concentration was collected at 65g / L, the pH was 7, the time was 1500h, no discoloration and rust was excellent, otherwise it was unqualified; the results are shown in Table 1;

[0087] Table 1

[0088]

[0089]

[0090] The invention provides a low-carbon steel hot-pressed thin plate and a preparation process thereof. By controlling process parameters, the low-carbon steel plate is subjected to hot pressing, quenching and annealing treatments in sequence to obtain a high-flatness thin plate, which is then subjected to micro-arc oxidation treatment to in-situ grow an alumina ceramic layer on the surface of the steel plate, and then coated with a sealing liquid prepared by modified nano-alumina and a photocurable aqueous polyurethane composite emulsion, and subjected to photocuring treatment to obtain a hot-pressed thin plate having excellent corrosion resistance, antibacterial properties and hydrophobicity.

[0091] Example 3 is compared with Comparative Examples 1 and 3. By controlling the process parameters of micro-arc oxidation treatment, an alumina ceramic layer with uniform pores is formed on a low-carbon steel hot-pressed thin plate, and then modified nano-alumina is introduced into the sealing liquid as a filler to fill the pores, thereby improving the bonding strength between the sealing liquid and the pretreated thin plate and improving its corrosion resistance at the same time; wherein the modified nano-alumina is nano-alumina grafted with 3-(isomethacryloyloxy)propyltrimethoxysilane and an organosilicon quaternary ammonium salt monomer, and 3-(isomethacryloyloxy)propyltrimethoxysilane The introduction of gives it an unsaturated double bond, so that it participates in the cross-linking complexity of the film layer formed by the sealing liquid under the action of a photoinitiator, thereby making the modified nano-alumina firmly adhere to the sealing layer formed by the sealing liquid; the organosilicon quaternary ammonium salt monomer is prepared by synthesizing N-(2-(dimethylamino)ethyl)-naphthaleneimide from 1,8-naphthalene anhydride and N,N-dimethylethylenediamine, and then quaternizing it with 3-chloropropyltrimethoxysilane, wherein naphthaleneimide is a naphthalene-containing hydrophobic group, which can more effectively improve the bactericidal property of the quaternary ammonium salt than the benzene-containing hydrophobic group, and improve its antibacterial and antifouling ability.

[0092] Example 3 is compared with Comparative Example 2 and Comparative Example 3. The present invention adopts UV curing, an environmentally friendly curing technology with low energy consumption and fast curing speed, to form a protective sealing layer on the surface of the hot-pressed thin plate. In order to overcome the problems of oxygen inhibition and uneven crosslinking that are easily generated in the existing UV curing process, the present invention is based on the concept of green environmental protection. The polyhydroxy bio-based polyol generated by the ring-opening agent polyethylene glycol after the epoxidized soybean oil of the cheap biomaterial is opened is used as the polyol and 1,4-butanediol and isophorone diisocyanate as raw materials, and the diisocyanate is used as the raw material. Hydroxymethylpropionic acid is used as a hydrophilic chain extender and bisphenol A diglycidyl ether is used as a modifier. Under the action of catalysts stannous octoate and dibutyltin dilaurate, a bio-based polyurethane prepolymer is generated. Pentaerythritol triacrylate is used as a capping agent. At the same time, a silicone quaternary ammonium salt monomer is introduced as an antibacterial agent. Deionized water is added for emulsification and the prepolymer is mixed with a photoinitiator to prepare a photocurable water-based polyurethane composite emulsion. A complex cross-linked network is constructed with modified nano-alumina, thereby greatly improving the corrosion resistance, antibacterial resistance, and hydrophobicity, and extending the service life of the hot-pressed thin plate.

[0093] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the present invention specification under the inventive concept of the present invention, or direct / indirect applications in other related technical fields, are included in the patent protection scope of the present invention.

Claims

1. A process for preparing a low carbon steel hot pressed sheet, characterized in that: The following steps are involved: S1: hot pressing, quenching, and tempering the low-carbon steel plate in sequence, and then alkali washing, acid washing, water washing, and alcohol washing in sequence after cleaning, and drying to obtain a hot pressed thin plate; S2: performing micro-arc oxidation treatment on the hot pressed thin plate to obtain a pre-treated thin plate having an alumina ceramic layer on the surface; S3: preparing sealing liquid using modified nano-alumina and photocurable waterborne polyurethane composite emulsion; S4: coating the sealing liquid on the surface of the pretreated thin plate, photocuring, and drying to obtain a low-carbon steel hot-pressed thin plate.

2. The process for preparing a low carbon steel hot pressed sheet according to claim 1, characterized in that: The working conditions of the hot pressing treatment are: keeping warm at 480°C for 3 hours and keeping warm at 420°C for 2 hours.

3. The process for preparing a low carbon steel hot pressed sheet according to claim 1, characterized in that: The working conditions of quenching treatment are: keeping at 800℃ for 5 minutes and cooling with oil; the working conditions of tempering treatment are: keeping at 400℃ for 1 hour and cooling with the furnace.

4. The process for preparing a low carbon steel hot pressed sheet according to claim 1, characterized in that: The working conditions of micro-arc oxidation treatment are: forward voltage of 540V, pulse frequency of 1450Hz, forward duty cycle of 15%, negative voltage of 50V, positive-negative pulse ratio of 1:1, and power-on time of 30min; the composition of the electrolyte used for micro-arc oxidation is: deionized water as solvent, containing 4-6g / L sodium aluminate, 0.5-1.5g / L disodium hydrogen phosphate, 0.5-1.5g / L sodium carbonate, 0.5-1.5g / L sodium tetraborate, and 1-3mL / L glycerol.

5. The process for preparing a low carbon steel hot pressed sheet according to claim 1, characterized in that: The mass ratio of the modified nano-alumina and the photocurable waterborne polyurethane composite emulsion in the sealing liquid is 15-17%.

6. The process for preparing a low carbon steel hot pressed sheet according to claim 1, characterized in that: The preparation of the modified nano-alumina comprises the following steps: (1) 1,8-naphthalene anhydride, N,N-dimethylethylenediamine and anhydrous ethanol are mixed, stirred for 3-4 hours, and subjected to rotary evaporation. The mixture is purified by silica gel column using a dichloromethane and methanol in a volume ratio of 10:1 as an eluent to obtain N-(2-(dimethylamino)ethyl)-naphthaleneimide; (2) Under nitrogen protection, 3-chloropropyltrimethoxysilane, N-(2-(dimethylamino)ethyl)-naphthaleneimide and toluene are mixed, kept at 78-82° C. for 33-36 hours, and rotary evaporated to obtain an organosilicon quaternary ammonium salt monomer; (3) 3-(isobutyleneoxy)propyltrimethoxysilane, organosilicon quaternary ammonium salt monomer and deionized water are mixed, the pH value is adjusted to 4, a mixed solution of nano-alumina and anhydrous ethanol is added, the temperature is raised to 58-62° C. and kept warm for 2-3 hours, and the mixture is washed, dried and ground to obtain modified nano-alumina.

7. The process for preparing a low carbon steel hot pressed sheet according to claim 6, characterized in that: The mass ratio of the 3-(isomethacryloyloxy)propyltrimethoxysilane, the organosilicon quaternary ammonium salt monomer and the nano-alumina is 2:1:

3.

8. The process for preparing a low carbon steel hot pressed sheet according to claim 1, characterized in that: The preparation of the photocurable aqueous polyurethane composite emulsion comprises the following steps: 1) Under a nitrogen atmosphere, polyethylene glycol and epoxidized soybean oil are mixed, concentrated sulfuric acid is added, and the mixture is kept in an oil bath at 98-102° C. for 2-3 hours, sodium carbonate solution is added, the mixture is cooled, ethyl acetate is added, the mixture is washed with saturated sodium chloride water, dried with anhydrous magnesium sulfate, filtered, and rotary evaporated to obtain a polyhydroxy bio-based polyol; 2) In a nitrogen atmosphere, polyhydroxy bio-based polyol, 1,4-butanediol and isophorone diisocyanate are mixed, heated to 68-72°C and kept warm for 1-2 hours, cooled to 42-45°C, acetone is added, dimethylol propionic acid and bisphenol A diglycidyl ether are added, heated to 48-52°C, stannous octoate and dibutyltin dilaurate are added and kept warm for 3-4 hours, pentaerythritol triacrylate is added and kept warm for 1-2 hours, a mixture of organosilicon quaternary ammonium salt monomer and deionized water is added, triethylamine is added and kept warm for 20-30 minutes, deionized water is added for emulsification for 1 hour, rotary evaporation is performed, a photoinitiator is added, and a photocurable waterborne polyurethane composite emulsion is obtained.

9. The process for preparing a low carbon steel hot pressed sheet according to claim 8, characterized in that: The mass ratio of polyhydroxy bio-based polyol, 1,4-butanediol, isophorone diisocyanate, dihydroxymethylpropionic acid, bisphenol A diglycidyl ether, pentaerythritol triacrylate, and silicone quaternary ammonium salt monomer is 1.8:0.12:2:0.15:0.15:0.33:0.

8.

10. A low carbon steel hot pressed sheet, characterized in that: The invention is prepared by the preparation process according to any one of claims 1 to 9.

Citation Information

Cited By

  • High-thermal-conductivity anti-corrosion hydrophilic aluminum foil and preparation method thereof

    CN119842309A

  • Corrosion-resistant high-tensile zinc alloy material and preparation process thereof

    CN121320757A