Gallium oxide single crystal growth device and method

Through the crucible-free gallium oxide single crystal growth device, high-frequency alternating magnetic field suspension heating technology, combined with zone melting method and suspension smelting process, the high cost and pollution problems of precious metal crucibles are solved, and the efficient growth of large-size gallium oxide single crystals is achieved. , meet industrial needs.

CN118932478AActive Publication Date: 2024-11-12HANGZHOU GAREN SEMICON CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411434996.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-15
Publication Date
2024-11-12
Estimated Expiration
2044-10-15

AI Technical Summary

Technical Problem

The existing gallium oxide single crystal growth technology has high cost and pollution problems of precious metal crucibles, and traditional crucible-free processes are difficult to grow large-sized single crystals, which cannot meet the needs of industrialization.

Method used

The crucible-free gallium oxide single crystal growth device is adopted, and a high-frequency alternating magnetic field is provided by a spiral induction coil. The suspended heat source is stably suspended and heated in the magnetic field. Combined with the zone melting method and suspension melting process, the growth of large-sized gallium oxide single crystals is achieved. .

Benefits of technology

It avoids the high cost and impurity pollution of precious metal crucibles, meets the growth needs of large-sized gallium oxide single crystals above 2 inches, reduces production costs, and improves the purity and performance of the crystals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932478A_ABST
    Figure CN118932478A_ABST
Patent Text Reader

Abstract

The invention provides a gallium oxide single crystal growth device and method, and the device comprises a furnace body, an upper seed rod penetrating through an upper cover, a lower seed rod penetrating through a lower cover, and a spiral induction coil wound on the periphery of a furnace cylinder, and is used for providing a high-frequency alternating magnetic field; the induction coil comprises a stabilizing coil and a suspension heating coil from top to bottom, the direction of electromagnetic force generated after the stabilizing coil is electrified is opposite to that of electromagnetic force generated after the suspension heating coil is electrified, and the stabilizing coil and the suspension heating coil interact with each other, so that a suspension heat source put in the furnace barrel stably suspends in a working area defined by the induction coil in a working state. According to the method, an induction coil is used for heating a suspension heat source, then the suspension heat source is used for heating a charge bar to obtain a suspension melt, seed crystals make contact with the suspension melt, growth of the gallium oxide single crystal is completed, and the requirement for growing the large-size gallium oxide single crystal with the size being 2 inches or above without a crucible is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of gallium oxide single crystal growth, and in particular to a gallium oxide single crystal growth device and method. Background Art

[0002] Gallium oxide (β-Ga2O3) is a new generation of ultra-wide bandgap semiconductor material with the advantages of large bandgap width (4.85 eV), high breakdown electric field strength (8 MV / cm), large Baliga quality factor and stable physical and chemical properties. Studies have shown that its Baliga's Figure of Merit (BFOM) is about 3400 times that of Si and about 10 times that of SiC. It can reduce the power loss of electronic devices during use and has great application value in power devices, optoelectronic devices, sensors and other fields. It is one of the important substitutes for wide bandgap semiconductor materials silicon carbide and gallium nitride.

[0003] At present, conventional methods for growing gallium oxide (β-Ga2O3) single crystals include processes that require the use of crucibles and traditional crucible-free processes. Processes that require the use of crucibles include the Czochralski method, the guided mold method, the Bridgman method, the casting method, etc. The crucibles used in these growth processes are made of the precious metal iridium, and its material cost is difficult to reduce; and during the growth of gallium oxide single crystals, the iridium crucible will be corroded and worn, further increasing the production cost. More importantly, gallium oxide single crystals will be doped and contaminated by iridium during growth, affecting the purity of the crystals and, in turn, the performance of the crystals. Although traditional crucible-free processes such as the optical floating zone method do not require the use of precious metal crucibles, they can only grow gallium oxide single crystals less than 2 inches, which cannot meet the industry's needs for large quantities and large sizes.

[0004] In summary, if we want to meet the industrialization needs of gallium oxide single crystals, we urgently need to develop a crucible-free growth process and equipment that can grow large-size gallium oxide single crystals. Summary of the invention

[0005] Based on this, in response to the above needs, the present invention proposes a crucible-free gallium oxide single crystal growth method and device, which can be used to grow large-size gallium oxide single crystals of more than 2 inches.

[0006] The gallium oxide single crystal growth device provided in the embodiment of the present application includes: A gallium oxide single crystal growth device includes: A furnace body, the furnace body comprises a furnace barrel, an upper cover and a lower cover respectively arranged at both ends of the furnace barrel, the upper cover is provided with a feeding channel and a first gas channel connected to the interior of the furnace barrel, the feeding channel is used to feed suspended heat source materials into the furnace barrel, and the lower cover is provided with a second gas channel connected to the interior of the furnace barrel; in a working state, the first gas channel and the second gas channel serve as an air inlet channel and an air outlet channel respectively, so that a stable gas atmosphere is formed in the furnace body. Preferably, the first gas channel is an air outlet channel, and the second gas channel is an air inlet channel.

[0007] An upper seed crystal rod passing through the upper cover, the upper seed crystal rod being used to place a gallium oxide material rod; A lower seed crystal rod passing through the lower cover, wherein the lower seed crystal rod is used to place gallium oxide seed crystals; The spiral induction coil wound around the outer periphery of the furnace drum is used to provide a high-frequency alternating magnetic field; the induction coil includes a stabilizing coil and a suspension heating coil from top to bottom, the stabilizing coil generates a first downward electromagnetic force when energized, and the suspension heating coil generates a second upward electromagnetic force when energized, the first electromagnetic force and the second electromagnetic force interact with each other so that the suspension heat source placed in the furnace drum is stably suspended in the working area surrounded by the induction coil in the working state.

[0008] Preferably, the winding direction of the stabilizing coil is opposite to that of the suspension heating coil, so that in the working state, the suspension heat source located in the working area is subjected to electromagnetic forces from the stabilizing coil and the suspension heating coil in opposite directions and check and balance each other to maintain the suspension heat source stably suspended in the working area without moving up and down due to uneven force.

[0009] Preferably, the metal pipe around which the induction coil is wound is a hollow structure, and the metal pipe around which the stabilizing coil is wound is connected to the metal pipe around which the suspension heating coil is wound. In the working state, coolant can be passed into the hollow structure of the induction coil to maintain the induction coil in a state where the temperature rises due to high-power energization, and the induction coil can still work normally without being damaged. In addition, the metal pipe around which the stabilizing coil is wound is connected to the metal pipe around which the suspension heating coil is wound, and only one liquid inlet and one liquid outlet are needed to complete the passage of coolant into the entire induction coil, and the coolant can be continuously passed into and out of the metal pipe.

[0010] Preferably, the suspension heating coil includes a heating coil and a suspension coil from top to bottom, the heating coil is cylindrically wound, the suspension coil is inverted cone-shaped, and the setting range of the semi-cone angle β of the suspension coil is 0°<β≤90°. In the working state, the main function of the heating coil is to continuously heat the suspension heat source while providing an upward second electromagnetic force for the suspension heat source, so as to continuously melt the gallium oxide material rod; and the main function of the suspension coil is to continuously provide an upward second electromagnetic force for the suspension heat source, so as to stably suspend the suspension heat source. Moreover, when the number of winding turns and the vertical spacing of the turns are the same, the electromagnetic force provided by the suspension coil in inverted cone shape is greater than that of the cylindrical winding. The suspension coil in inverted cone shape can also control the shape of the suspension heat source to be inverted cone shape, which is convenient for accelerating the speed at which the molten gallium oxide material rod flows onto the seed crystal, and the contact area with the seed crystal is easy to control, which is convenient for accelerating and optimizing the formation process of the gallium oxide single crystal.

[0011] Preferably, the number of turns of the stabilizing coil is N1, the number of turns of the heating coil is N2, and the number of turns of the suspension coil is N3, wherein N1≤N2, and N1≤N3. The more turns of the coil, the greater the magnetic field strength and electromagnetic force generated when powered on. In the working state, since the first electromagnetic force provided by the stabilizing coil is directed downward, which is the same as the gravity direction of the suspended heat source, if the suspended heat source is to be kept in a stable suspended state, the number of turns of the stabilizing coil needs to be controlled to be smaller than the number of turns of the suspension coil; and since the direction of the magnetic field provided by the stabilizing coil is opposite to that of the heating coil, if the heating effect of the heating coil is to be ensured, the number of turns of the stabilizing coil needs to be controlled to be smaller than the number of turns of the heating coil.

[0012] Preferably, the vertical spacing of the turns of the stabilizing coil is d1, the vertical spacing of the turns of the heating coil is d2, and the vertical spacing of the turns of the suspension coil is d3, wherein d1≥d2, and d1≥d3. The smaller the vertical spacing of the turns of the coils, the greater the magnetic field strength and electromagnetic force generated when powered on. In the working state, since the first electromagnetic force provided by the stabilizing coil is directed downward, which is the same as the gravity direction of the suspension heat source, if the suspension heat source is to be kept in a stable suspension state, the vertical spacing of the turns of the stabilizing coil needs to be controlled to be greater than the vertical spacing of the turns of the suspension coil; and since the direction of the magnetic field provided by the stabilizing coil is opposite to that of the magnetic field of the heating coil, if the heating effect of the heating coil is to be ensured, the vertical spacing of the turns of the stabilizing coil needs to be controlled to be greater than the vertical spacing of the turns of the heating coil.

[0013] Preferably, d2≥d3. The smaller the vertical spacing between the turns of the suspension coil, the greater the suspension force (ie, the second electromagnetic force) provided to the suspension heat source, and the easier it is for the suspension heat source to form an inverted cone.

[0014] Preferably, the first gas channel is an outlet channel, and the second gas channel is an inlet channel. During operation, a gas channel is formed from bottom to top, so that the gas in the inlet channel with a lower temperature is preferentially contacted with the grown gallium oxide single crystal, which can accelerate the growth rate of the gallium oxide single crystal on the one hand, and on the other hand, during the crystal growth process, the gallium oxide material rod and the suspended heat source area require high temperature, and during the bottom-up ventilation process, the gas temperature can be gradually increased, thereby reducing the effect of the gas temperature on the temperature of the gallium oxide material rod and the suspended heat source area.

[0015] Preferably, the furnace barrel is a sapphire barrel or a quartz barrel. Since the induction coil is wound outside the furnace barrel, and in the process of heating the suspended heat source, the light in the infrared band plays a heating role, the embodiment of the present application gives priority to selecting materials that are transparent to the infrared band, that is, the furnace barrel material allows infrared light to pass through, and does not absorb or reflect most of the infrared light, and the furnace barrel material has a high melting point and does not react with the gas introduced during the working process, thereby ensuring the stability of the gallium oxide single crystal growth process.

[0016] Preferably, the diameter of the gallium oxide single crystal grown by the gallium oxide single crystal growth device is D, and the inner diameter of the furnace drum is within the range of 1.2D-3D, thereby providing sufficient space for the growth of the gallium oxide single crystal.

[0017] The embodiment of the present invention further discloses a gallium oxide single crystal growth method, using the gallium oxide single crystal growth device described above, the growth method comprising: Installing a gallium oxide material rod on the upper seed crystal rod, and installing a gallium oxide seed crystal on the lower seed crystal rod; A first flowing gas is introduced into the furnace barrel through the first gas channel and the second gas channel to form a stable flowing atmosphere in the furnace barrel; An alternating current of a preset frequency and a preset magnitude is passed through the induction coil to form a high-frequency alternating magnetic field of a target frequency and a target power in a working area enclosed by the induction coil in the furnace drum; A suspended heat source material is fed into the furnace drum through the feeding channel. Under the action of the high-frequency alternating magnetic field, the stabilizing coil generates a first downward electromagnetic force after being energized, and the suspended heating coil generates a second upward electromagnetic force after being energized. The first electromagnetic force and the second electromagnetic force interact with each other to melt the suspended heat source material in the working area to obtain a suspended heat source, and the suspended heat source is stably suspended in the working area. The suspended heat source material is a conductive material, the working temperature of the suspended heat source is T1, the melting point of the gallium oxide material rod is T2, and T1>T2; Entering the feeding stage: the upper seed crystal rod descends at a first speed V1, so that the bottom end of the gallium oxide material rod approaches and contacts the suspension heat source, so that the gallium oxide material rod is heated and melted, and the upper seed crystal rod is continuously descended until the molten gallium oxide material rod material completely wraps the suspension heat source to form a suspension melt (that is, the core of the suspension melt is the suspension heat source in a molten state, and the outer layer is the molten gallium oxide material rod material), and the suspension melt remains suspended under the action of the high-frequency alternating magnetic field; Stop introducing the first flowing gas, start introducing the second flowing gas, and form a stable flowing atmosphere; Entering the crystal growth stage: raising the lower seed crystal rod so that the top of the gallium oxide seed crystal approaches and contacts the bottom of the suspended melt, adjusting the descending rate of the lower seed crystal rod so that the gallium oxide single crystal starts to grow along the top of the gallium oxide seed crystal until the grown gallium oxide single crystal reaches a target size, continuing to descend the lower seed crystal rod so that the generated gallium oxide crystal is separated from the suspended melt, and then the upper seed crystal rod stops descending; during the growth of the gallium oxide single crystal, the upper seed crystal rod continues to descend so that the gallium oxide material rod continues to melt and maintain the state of the suspended melt, and the second flowing gas continues to flow into the furnace barrel; Entering the shutdown stage: maintaining the suspended melt state and continuing to suspend, stopping the introduction of the second flowing gas, and starting the introduction of the first flowing gas, until the molten gallium oxide rod material wrapping the suspended heat source in the suspended melt is volatilized and decomposed, stopping the introduction of the first flowing gas, starting the introduction of the second flowing gas, and gradually reducing the power of the induction coil to zero, so that the suspended heat source is oxidized and cooled to form a solid block and fall; when the furnace drum temperature drops to the target temperature, stopping the introduction of the second flowing gas.

[0018] Preferably, the crystal growth stage includes a seeding stage, a necking stage, a shoulder release stage, an equal diameter stage, and a finishing stage, and the process of each stage is: Seeding stage: the lower seed crystal rod rises at a second rate V2, so that the top of the gallium oxide seed crystal is close to and below the suspended melt; Neck shrinking stage: the lower seed crystal rod descends at a third rate V3, so that the gallium oxide single crystal begins to grow along the top of the gallium oxide seed crystal and forms a thin neck. During this process, the upper seed crystal rod continues to descend to melt the gallium oxide material rod and maintain the state of the suspended melt; Shoulder release stage: the lower seed crystal rod descends at a fourth rate V4, and / or the power of the induction coil is reduced to expand the diameter of the grown gallium oxide single crystal. During this process, the upper seed crystal rod continues to descend to melt the gallium oxide material rod and maintain the state of the suspended melt, wherein V4<V3; Equal diameter stage: when the diameter of the grown gallium oxide single crystal is expanded to the target size, the lower seed crystal rod descends at a fifth rate V5 to maintain the diameter of the grown gallium oxide single crystal at the target size. During this process, the upper seed crystal rod continues to descend to melt the gallium oxide material rod and maintain the state of the suspended melt, wherein V5<V4; Finishing stage: when the length of the grown gallium oxide single crystal reaches the target size, the lower seed crystal rod descends at a sixth rate V6, and / or the power of the induction coil is increased, so that the diameter of the grown gallium oxide single crystal gradually decreases until it is separated from the suspended melt. When the gallium oxide single crystal is separated from the suspended melt, the upper seed crystal rod stops descending, wherein V6>V5.

[0019] Preferably, the first flowing gas is an inert gas, the second flowing gas is a mixed gas containing oxygen and other gases, the other gases include one or more of carbon dioxide, argon, and nitrogen, and the oxygen content in the second flowing gas is X, 0<X≤100%.

[0020] Preferably, the flow rate of the first flowing gas is equal to the flow rate of the second flowing gas.

[0021] Preferably, the suspended heat source material has good electrical conductivity and a boiling point higher than the melting point of the gallium oxide material rod. The suspended heat source material has low reactivity or a low solid solubility limit with the molten gallium oxide material rod material, and does not change the electrical type of the gallium oxide single crystal in the molten state.

[0022] Preferably, when the electrical type of the gallium oxide single crystal is n-type, the suspended heat source material is Sn, Si, Ta or Nb; when the electrical type of the gallium oxide single crystal is semi-insulating, the suspended heat source material is Fe or Mg; when the electrical type of the gallium oxide single crystal is unintentionally doped, the suspended heat source material is Ga.

[0023] Preferably, the operating temperature T1 of the suspended heat source is in the range of 1750°C-1900°C.

[0024] Preferably, the diameter of the side of the suspended heat source in contact with the gallium oxide material rod is D1, the diameter of the gallium oxide material rod is D2, and the diameter of the gallium oxide single crystal is D3, wherein D1≥D2, and D3≥D2.

[0025] Preferably, the shape of the suspended heat source is an inverted cone, the bottom diameter of the suspended heat source is D1, the weight is m, the density is ρ, Where, D1=(24m×tanβ / (πρ))^(1 / 3); Alternatively, the suspended heat source is spherical or cylindrical in shape.

[0026] Preferably, the weight m of the suspended heat source is within 1g-100g.

[0027] Preferably, during operation, the frequency of the induction coil is within 1 kHz-500 kHz, the power of the induction coil is within 1 kW-2000 kW, and the frequency of the induction coil remains unchanged during operation.

[0028] Preferably, in the equal diameter stage, the descending rate V5 of the lower seed crystal rod is within 0.5 mm / h-50 mm / h to ensure that the diameter size of the grown gallium oxide single crystal is uniform.

[0029] Preferably, the diameter of the gallium oxide single crystal is within a range of 2 inches to 8 inches.

[0030] The crucible-free gallium oxide single crystal growth method and device proposed in the embodiments of the present application are no longer limited by the high cost of precious metal crucibles, and also avoid the contamination of gallium oxide single crystals by precious metal impurities. At the same time, it is no longer limited by the heating light source of the optical floating zone method, and can meet the growth requirements of large-size gallium oxide single crystals of more than 2 inches.

[0031] Specifically, the spiral induction coil wound around the outer periphery of the furnace drum provides a high-frequency alternating magnetic field when powered on, wherein the downward first electromagnetic force generated by the stabilizing coil in the induction coil and the upward second electromagnetic force generated by the suspension heating coil interact with each other, so that the suspension heat source material fed into the furnace drum through the feeding channel above the furnace drum can be stably suspended in the working area surrounded by the induction coil in the working state, and the suspension heating coil can also heat the suspension heat source material to melt the suspension heat source material to obtain a suspension heat source, and keep the suspension heat source in a molten working state during the entire crystal growth process. Later, during the crystal growth process, the suspension heat source in a molten state is used as a heat source to contact the gallium oxide material rod installed on the upper seed crystal rod, heat the gallium oxide material rod, and melt the gallium oxide material rod and completely wrap the suspension heat source to form a suspension melt, that is, the core of the suspension melt is the suspension heat source in a molten state, and the outer layer is the molten gallium oxide material rod material. After obtaining the suspended melt, the upper seed crystal rod is continuously lowered to allow the material rod to continue to melt, and the lower seed crystal rod is raised at the same time to allow the gallium oxide seed crystal to contact the suspended melt, and the crystal growth process is started. This crystal growth process is similar to the crystal growth process of the zone melting method, until the gallium oxide single crystal of the target size is obtained, and then the furnace is shut down. Since the molten gallium oxide material rod material is easy to volatilize in an oxygen-deficient atmosphere, the present application first creates an oxygen-deficient atmosphere in the furnace drum to volatilize the molten gallium oxide material rod material of the outer layer of the suspended melt, and since the suspended heat source material can be oxidized to form an oxide solid in an oxidizing atmosphere, the oxide has poor conductivity, and the electromagnetic suspension force it is subjected to becomes smaller, so that it can gradually fall to the bottom of the furnace drum for removal.

[0032] The embodiment of the present application can adjust the size of the suspended heat source within the range allowed by the heating power borne by the induction coil, so that gallium oxide single crystal rods of different sizes can be generated as needed, and large-sized gallium oxide single crystal rods can be generated. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 is a cross-sectional structural diagram of a gallium oxide single crystal growth device in one embodiment; Figure 2 This is a flow chart of a method for growing a gallium oxide single crystal in one embodiment; Figure 3 This is a flow chart of a method for growing a gallium oxide single crystal in one embodiment; Figure 4 is a cross-sectional schematic diagram of a gallium oxide single crystal growth device in a working process in one embodiment; Figure 5 Schematic diagram of the current direction of the induction coil during the growth of a gallium oxide single crystal in one embodiment.

[0034] Explanation of reference numerals: 11. furnace drum; 12. upper cover; 13. feeding channel; 14. first gas channel; 15. lower cover; 16. second gas channel; 2. upper seed crystal rod; 21. gallium oxide material rod; 22. suspended melting zone; 23. molten pool; 3. lower seed crystal rod; 31. gallium oxide seed crystal; 4. induction coil; 41. stabilizing coil; 42. heating coil; 43. suspension coil; 5. suspension heat source; 6. gallium oxide single crystal. DETAILED DESCRIPTION

[0035] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0036] As described in the background technology, the methods for growing gallium oxide single crystals in the prior art all have shortcomings. Therefore, the embodiments of the present application provide a crucible-free gallium oxide single crystal growth method and device, which cleverly combine the advantages of the zone melting method and the suspension melting process. It is no longer limited by the high cost of precious metal crucibles in the growth process that requires a crucible in the prior art, and also avoids the contamination of gallium oxide single crystals by precious metal impurities. At the same time, it is no longer limited by the limitations of the crucible-free process in the prior art on the size of gallium oxide single crystals. For example, it is no longer limited by the limitations of the heating light source of the optical floating zone method, and can meet the growth requirements of large-sized gallium oxide single crystals of more than 2 inches.

[0037] Specifically, Figure 1 FIG. 1 is a schematic diagram of a cross-sectional structure of a gallium oxide single crystal growth device disclosed in an embodiment of the present application. The growth device structure includes: The furnace body includes a furnace barrel 11, an upper cover 12 and a lower cover 15 respectively arranged at the upper and lower ends of the furnace barrel 11, the upper cover 12 is provided with a feeding channel 13 and a first gas channel 14 connected to the interior of the furnace barrel 11, the feeding channel 13 is used to feed suspended heat source materials into the furnace barrel 11, and the lower cover 15 is provided with a second gas channel 16 connected to the interior of the furnace barrel 11. Furthermore, the first gas channel 14 and the second gas channel 16 are used to provide a stable gas atmosphere during the growth of the gallium oxide single crystal, that is, one of them serves as an inlet channel and the other as an outlet channel. In order to improve the growth efficiency of the gallium oxide single crystal and to avoid the influence of impurities in the furnace barrel on the quality of the gallium oxide single crystal, the present application preferably uses the second gas channel 16 as the inlet channel and the first gas channel 14 as the outlet channel, that is, in the actual production process, a flowing gas atmosphere from bottom to top is formed in the furnace barrel.

[0038] In addition, since the induction coil is wound outside the furnace drum, and in the process of heating the suspended heat source, the light in the infrared band plays a heating role, the embodiment of the present application gives priority to selecting materials that are transparent to the infrared band in terms of the selection of the furnace drum material, that is, the furnace drum material allows infrared light to pass through, and does not absorb or reflect most of the infrared light, and the furnace drum material has a high melting point and does not react with the gas introduced during the working process, thereby ensuring the stability of the gallium oxide single crystal growth process. In this embodiment, the furnace drum 11 is preferably a sapphire drum or a quartz drum.

[0039] Furthermore, the diameter of the gallium oxide single crystal grown by the gallium oxide single crystal growth device is D, and the inner diameter of the furnace drum is within the range of 1.2D-3D, that is, the inner diameter of the furnace drum needs to be larger than the diameter of the gallium oxide single crystal, so as to reserve sufficient space for high-temperature expansion of the furnace drum under high-temperature working conditions. Furthermore, since a stable flow atmosphere needs to be maintained inside the furnace drum during the entire gallium oxide growth process, in order to leave enough space for gas to pass through and avoid the gas flow being blocked by crystals in the furnace drum and causing a furnace explosion accident, the inner diameter of the furnace drum also needs to be set larger than the diameter of the gallium oxide single crystal.

[0040] The growth device also includes an upper seed crystal rod 2 that penetrates the upper cover 12, and the upper seed crystal rod 2 is used to place a gallium oxide material rod. The gallium oxide material rod used to grow a gallium oxide single crystal is generally a polycrystalline material rod with an irregular crystal sequence arrangement, and in this application, it can be a polycrystalline ceramic rod formed by pressing and sintering gallium oxide powder. In actual production, the gallium oxide material rod can be installed on the upper seed crystal rod 2 in a conventional manner, such as by clamping, threading, clamping with a clamping mechanism, etc., as long as the stability of the material rod is maintained during the growth of the gallium oxide single crystal.

[0041] The lower seed crystal rod 3 is passed through the lower cover 15, and the lower seed crystal rod 3 is used to place the gallium oxide seed crystal. The electrical properties of the generated gallium oxide single crystal are affected by the electrical properties of the gallium oxide seed crystal and the impurities doped in the gallium oxide material rod. In actual production, it is necessary to select a gallium oxide seed crystal with the same electrical properties as the gallium oxide single crystal to be generated. The method of mounting the gallium oxide seed crystal on the lower seed crystal rod 3 can be the same as the method of mounting the gallium oxide material rod on the upper seed crystal rod 2, or it can be different, as long as the stability of the gallium oxide seed crystal is maintained during the growth of the gallium oxide single crystal.

[0042] The spiral induction coil 4 wound around the outer periphery of the furnace drum 11 is used to provide a high-frequency alternating magnetic field; the induction coil 4 includes a stabilizing coil and a suspension heating coil from top to bottom. The stabilizing coil generates a first downward electromagnetic force F1 when energized, and the suspension heating coil generates a second upward electromagnetic force F2 when energized. The first electromagnetic force and the second electromagnetic force interact with each other so that the suspension heat source placed in the furnace drum is stably suspended in the working area enclosed by the induction coil when in a working state.

[0043] In the actual production process, the magnitude of the second electromagnetic force F2 must be equal to the sum of the gravity G of the suspended heat source and the magnitude of the first electromagnetic force F1 to maintain the suspended heat source in the working area. The first electromagnetic force F1 provided by the stabilizing coil can be used to stabilize and limit the position of the suspended heat source to prevent the suspended heat source from swinging up and down during operation.

[0044] It can be understood that, in addition to providing the second electromagnetic force F2, the function of the suspension heating coil is to provide thermal energy for heating the suspension heat source.

[0045] In this embodiment, the winding direction of the stabilizing coil is opposite to that of the suspension heating coil, so that in the working state, the suspension heat source located in the working area is subjected to electromagnetic forces from the stabilizing coil and the suspension heating coil in opposite directions and check and balance each other to maintain the suspension heat source stably suspended in the working area without moving up and down due to uneven force.

[0046] Further, in other embodiments, the suspension heating coil includes a top-down heating coil and a suspension coil, such as Figure 5As shown, the induction coil 4 is divided from top to bottom into a stabilizing coil 41 at the top, a heating coil 42 in the middle, and a suspension coil 43 at the bottom. The stabilizing coil 41 is preferably wound in a cylindrical shape, the heating coil 42 is also wound in a cylindrical shape, and the suspension coil 43 is wound in an inverted cone shape. The setting range of the semi-cone angle β of the suspension coil is 0°<β≤90°. Since the current direction in the stabilizing coil 41 needs to be opposite to the current direction in the heating coil 42 and the suspension coil 43 in the working state, in order to reduce the setting of multiple current input structures, the winding direction of the stabilizing coil 41 in the embodiment of the present application is opposite to the winding direction of the heating coil 42 and the suspension coil 43.

[0047] In the working state, the main function of the heating coil is to continuously heat the suspended heat source while providing an upward second electromagnetic force to the suspended heat source so as to continuously melt the gallium oxide rod; and the main function of the suspension coil is to continuously provide an upward second electromagnetic force to the suspended heat source so as to stably suspend the suspended heat source. Moreover, when the number of winding turns and the vertical spacing of the turns are the same, the electromagnetic force provided by the suspension coil wound in an inverted cone shape is greater than that of the cylindrical winding. The suspension coil wound in an inverted cone shape can also control the shape of the suspended heat source to be an inverted cone shape, which is convenient for accelerating the speed at which the molten gallium oxide rod material flows to the seed crystal, and the inverted cone-shaped suspension heat source can also guide the flow path of the molten gallium oxide rod material, so that the contact area between the molten gallium oxide rod material and the seed crystal is easy to stably control, which is convenient for accelerating and optimizing the formation process of the gallium oxide single crystal.

[0048] It is understandable that during the growth of the gallium oxide single crystal, the role of the suspended heat source is mainly to heat and melt the gallium oxide rod. The shape of the suspended heat source can be arbitrary, as long as the surface lines are smooth and the molten gallium oxide rod material can be smoothly connected with the gallium oxide seed crystal or the molten pool 23 (see Figure 4 ) contact. In other facility examples, the shape of the suspension heat source can be cylindrical, spherical, ellipsoidal, etc. Correspondingly, the shape of the suspension heat source is controlled by the winding shape of the suspension coil. When the shape of the suspension heat source is cylindrical, the suspension coil is cylindrically wound, that is, the semi-cone angle β of the suspension coil is 90°. Similarly, when the shape of the suspension heat source is spherical, the suspension coil is spherically wound, that is, the winding diameter gradually increases from the upper end to the middle end and from the lower end to the middle end of the suspension coil. This embodiment does not give too many examples of the winding shape of the suspension coil. It is only necessary to adaptively adjust the winding shape of the suspension coil according to the shape of the suspension heat source.

[0049] Specifically, the number of turns of the stabilizing coil 41 is N1, the number of turns of the heating coil 42 is N2, and the number of turns of the suspension coil 43 is N3, wherein N1≤N2, and N1≤N3. The more turns of the coil, the greater the magnetic field strength and electromagnetic force generated when powered on. In the working state, since the first electromagnetic force provided by the stabilizing coil is directed downward, which is the same as the gravity direction of the suspension heat source, if the suspension heat source is to be kept in a stable suspension state, the number of turns of the stabilizing coil needs to be controlled to be smaller than the number of turns of the suspension coil; and since the direction of the magnetic field provided by the stabilizing coil is opposite to the direction of the magnetic field of the heating coil, if the heating effect of the heating coil is to be ensured, the number of turns of the stabilizing coil needs to be controlled to be smaller than the number of turns of the heating coil.

[0050] Furthermore, the vertical spacing of the turns of the stabilizing coil 41 is d1, the vertical spacing of the turns of the heating coil 42 is d2, and the vertical spacing of the turns of the suspension coil 43 is d3, wherein d1≥d2, and d1≥d3. The smaller the vertical spacing of the turns of the coils, the greater the magnetic field strength and electromagnetic force generated when powered on. In the working state, since the first electromagnetic force provided by the stabilizing coil is directed downward, which is the same as the gravity direction of the suspension heat source, if the suspension heat source is to be kept in a stable suspension state, the vertical spacing of the turns of the stabilizing coil needs to be controlled to be greater than the vertical spacing of the turns of the suspension coil; and since the direction of the magnetic field provided by the stabilizing coil is opposite to that of the magnetic field of the heating coil, if the heating effect of the heating coil is to be ensured, the vertical spacing d1 of the turns of the stabilizing coil needs to be controlled to be greater than the vertical spacing d2 of the turns of the heating coil.

[0051] Furthermore, the smaller the vertical spacing between the turns of the suspension coil is, the greater the suspension force (ie, the second electromagnetic force) provided for the suspension heat source is, and the easier it is for the suspension heat source to form an inverted cone shape. In the embodiment of the present application, d2≥d3 is preferably set.

[0052] It should be noted that the number of turns N3 and the vertical spacing d3 of the suspension coil are strongly related to the weight of the suspension heat source, and the weight of the suspension heat source is related to the diameter of the gallium oxide single crystal to be generated, that is, the larger the diameter of the gallium oxide single crystal to be generated, the greater the weight of the suspension heat source, the larger the number of turns N3 of the suspension coil, and the smaller the vertical spacing d3 of the turns. In addition, the number of turns N2 and the vertical spacing d2 of the heating coil are also strongly related to the weight of the suspension heat source. The greater the weight of the suspension heat source, the greater the heat energy and power required to melt the suspension heat source material, the larger the number of turns N2 of the heating coil, and the smaller the vertical spacing d2 of the turns.

[0053] In the embodiment of the present application, there is no absolute size relationship between the number of turns N3 of the suspension coil and the number of turns N2 of the heating coil. Specifically, when the size of the gallium oxide single crystal to be generated is relatively small, the weight of the suspension heat source is also relatively small, and a large suspension force is not required. At this time, usually N3≤N2; when the size of the gallium oxide single crystal to be generated is relatively large, the weight of the suspension heat source is also relatively large, and a stronger suspension force is required. At this time, there may be a situation where N3≥N2.

[0054] Furthermore, in this embodiment, the metal pipe around which the induction coil is wound is a hollow structure, and the metal pipe around which the stabilizing coil is wound is connected to the metal pipe around which the suspension heating coil is wound. In the working state, a coolant (such as cooling water) can be passed into the hollow structure of the induction coil to maintain the induction coil in a state where the temperature rises due to the high-power energization, and the induction coil can still work normally without being damaged. In addition, the metal pipe around which the stabilizing coil is wound is connected to the metal pipe around which the suspension heating coil is wound, and only one liquid inlet and one liquid outlet are needed to complete the passage of coolant into the entire induction coil, and the coolant can be continuously passed into and out of the metal pipe.

[0055] It should be noted that, in order to conveniently control the growth process of the gallium oxide single crystal, it is also necessary to timely learn the growth state of the gallium oxide single crystal in the furnace drum 11. Therefore, in other embodiments, the gallium oxide single crystal growth device further includes: An observation window is arranged on the outer wall of the furnace drum to observe the crystal growth state in the furnace drum; The temperature sensor and pressure sensor arranged in the furnace barrel are used to understand and record the temperature and pressure conditions in the furnace barrel, so as to adjust the gas atmosphere in the furnace barrel in real time. The temperature sensor and the pressure sensor can be arranged on the inner wall of the furnace barrel, or on the side of the upper cover or the lower cover close to the inner wall of the furnace barrel, or in the air inlet channel and / or the air outlet channel, which is not limited in this embodiment; Weight sensors are provided on the upper seed crystal rod and the lower seed crystal rod to provide feedback on the consumption of the material rod and the crystal growth during the growth of the gallium oxide single crystal; In addition, it also includes a control system for receiving temperature signals, air pressure signals, weight signals of material rods and / or gallium oxide single crystals in the furnace, etc., and adaptively adjusting various parameters in the growth process of the gallium oxide single crystal to ensure smooth growth of the gallium oxide single crystal.

[0056] The gallium oxide single crystal growth device proposed in the embodiment of the present application does not require a precious metal crucible, and is no longer limited by the high cost of the precious metal crucible, and also avoids the contamination of the gallium oxide single crystal by precious metal impurities. At the same time, it is no longer limited by the heating light source of the optical floating zone method, and can meet the growth requirements of large-sized gallium oxide single crystals of more than 2 inches. The embodiment of the present application can adjust the size of the suspended heat source within the range allowed by the heating power borne by the induction coil, so that gallium oxide single crystal rods of different sizes can be generated on demand, and large-sized gallium oxide single crystal rods can be generated.

[0057] Another embodiment of the present application provides a method for growing a gallium oxide single crystal, such as Figure 2 As shown in FIG. 1 , it is a flow chart of the growth method. Figure 3 As shown, it is a cross-sectional schematic diagram of the working state of the gallium oxide single crystal growth device during the gallium oxide single crystal growth process. The growth method adopts the above embodiment as Figure 1 The gallium oxide single crystal growth device shown. Specifically, the growth method includes the following steps: Step S11: Install the gallium oxide rod 21 on the upper seed crystal rod 2, and install the gallium oxide seed crystal 31 on the lower seed crystal rod 3. As described in the above embodiments, various methods such as threaded installation and clamping can be used as long as the gallium oxide rod 21 and the gallium oxide seed crystal 31 are stably installed.

[0058] Step S12: introducing a first flowing gas into the furnace barrel through the first gas channel and the second gas channel to form a stable flowing atmosphere in the furnace barrel. Specifically, the air inlet channel of the lower cover and the air outlet channel of the upper cover in the sealed furnace body are opened, and the first flowing gas is introduced from bottom to top to form a stable flowing atmosphere.

[0059] It should be noted that a stable flow atmosphere means that the gas flows in one direction as a whole, which can be understood as the gas in the furnace being in a laminar state. In the laminar state, the movement of gas molecules along the flow direction presents a regular and parallel flow pattern. Specifically, the characteristics of laminar flow are: orderly flow: gas molecules flow along a fixed path without lateral mixing; parallel flow: all gas molecules flow in a direction parallel to the axis of the pipeline. In the embodiment of the present application, the gas flow in the furnace is preferably along the central axis of the furnace, flowing from bottom to top; no turbulence: no obvious vortex or irregular flow phenomenon.

[0060] As described in the above embodiments, the first gas channel 14 is an outlet channel, and the second gas channel 16 is an inlet channel. During operation, a gas channel is formed from bottom to top, so that the gas in the inlet channel with a lower temperature is preferentially in contact with the growing gallium oxide single crystal. On the one hand, the growth rate of the gallium oxide single crystal can be accelerated. On the other hand, during the crystal growth process, the gallium oxide material rod and the suspended heat source area require high temperature. During the bottom-up ventilation process, the gas temperature can be gradually increased, thereby reducing the effect of the gas temperature on the temperature of the gallium oxide material rod and the suspended heat source area.

[0061] Step S13: an alternating current of a preset frequency and a preset magnitude is passed through the induction coil to form a high-frequency alternating magnetic field of a target frequency and a target power in a working area enclosed by the induction coil in the furnace drum.

[0062] As described in the above embodiment, since the stabilizing coil 41 is wound in opposite directions to the heating coil 42 and the suspension coil 43, a high-frequency alternating magnetic field can be formed in the working area surrounded by the induction coil by simply passing an alternating current through the induction coil. Figure 5 As shown, it is an example of the current direction in the stabilizing coil 41, the heating coil 42 and the suspension coil 43. After the various parts of the induction coil are uniformly connected to the same AC power supply, since the winding directions of the stabilizing coil 41, the heating coil 42 and the suspension coil 43 are opposite, the current directions in the stabilizing coil 41, the heating coil 42 and the suspension coil 43 are also opposite.

[0063] During operation, considering the size of the gallium oxide single crystal to be generated and the weight of the suspended heat source, in this embodiment, it is preferred that the frequency of the induction coil is within 1 kHz-500 kHz, the power of the induction coil is within 1 kW-2000 kW, and the frequency of the induction coil remains unchanged during operation to maintain stable suspension of the suspended heat source.

[0064] In other embodiments, in order to ensure that the induction coil can maintain normal operation without being damaged when the temperature rises due to high-power energization, when AC current is passed through the induction coil, a coolant (such as cooling water) can be continuously passed into the hollow structure in the metal pipe of the induction coil in a timely manner according to the temperature rise of the induction coil to reduce the working temperature of the induction coil.

[0065] Step S14 : entering the feeding stage: namely, feeding the suspended heat source material into the furnace drum 11 through the feeding channel 13 .

[0066] Under the action of the high-frequency alternating magnetic field, the stabilizing coil 41 generates a first downward electromagnetic force after being energized, and the suspension heating coil generates a second upward electromagnetic force after being energized. The first electromagnetic force and the second electromagnetic force interact with each other to melt the suspension heat source material in the working area to obtain a suspension heat source 5, and the suspension heat source is stably suspended in the working area. The suspension heat source material is a conductive material.

[0067] Specifically, when the suspension heating coil is divided into a heating coil 42 and a suspension coil 43 from top to bottom, the heating coil 42 and the suspension coil 43 jointly provide an upward second electromagnetic force to overcome the gravity of the suspension heat source and suspend the suspension heat source, and the stabilizing coil 41 provides a downward first electromagnetic force to maintain the stable suspension of the suspension heat source. Under the joint action of the second electromagnetic force, the first electromagnetic force, and the gravity of the suspension heat source, the suspension heat source is kept stable and does not swing up and down. The heating coil 42 provides thermal energy for the suspension heat source material to melt the suspension heat source material, thereby obtaining the suspension heat source 5.

[0068] The suspension heat source material has good electrical conductivity so that it can be suspended under the action of electromagnetic force. The boiling point of the suspension heat source material is higher than the melting point of the gallium oxide material rod to ensure that the surface temperature of the suspension heat source in the molten state can melt the gallium oxide material rod. In addition, the suspension heat source material has low reactivity or low solid solubility limit with the molten gallium oxide material rod material, and does not change the electrical type of the gallium oxide single crystal in the molten state.

[0069] Furthermore, when the electrical type of the gallium oxide single crystal is n-type, the suspended heat source material is Sn, Si, Ta or Nb; when the electrical type of the gallium oxide single crystal is semi-insulating, the suspended heat source material is Fe or Mg; when the electrical type of the gallium oxide single crystal is unintentionally doped, the suspended heat source material is Ga.

[0070] It should be noted that the operating temperature of the suspension heat source is T1, the melting point of the gallium oxide rod is T2, T1>T2. The melting point T2 of the gallium oxide rod is between 1740℃ and 1900℃, so the operating temperature T1 of the suspension heat source is within the range of 1750℃-1900℃.

[0071] During operation, in order to ensure that the temperature in the furnace can be maintained at or above the melting point of the suspended heat source, the power of the induction coil is within 1kW-2000kW. In order to maintain the suspended state of the suspended heat source, the frequency of the induction coil is within 1kHZ-500kHZ, and the frequency of the induction coil remains unchanged during operation.

[0072] Step S15: Entering the feeding stage: the upper seed crystal rod 2 descends at a first rate V1, so that the bottom end of the gallium oxide material rod 21 approaches and contacts the suspended heat source 5, so that the gallium oxide material rod 21 is heated and melted, and the upper seed crystal rod is continuously descended until the molten gallium oxide material completely wraps the suspended heat source 5 to form a suspended melt, and the suspended melt remains suspended under the action of the high-frequency alternating magnetic field.

[0073] It should be noted that the core of the suspended melt is the suspended heat source 5 in a molten state, and the outer layer is the molten gallium oxide material (i.e., the suspended melt zone 22). After the suspended melt is formed, the surface layer of the suspended heat source 5 is wrapped by the molten gallium oxide material. At this time, the suspended heat source 5 will no longer be in contact with the gas atmosphere in the furnace, that is, when the oxygen-containing gas is introduced at this time, the suspended heat source 5 will not be oxidized. In addition, the gallium oxide material rod is usually a non-conductive material, and the gallium oxide material rod alone will not be suspended in the alternating magnetic field. Therefore, after the material rod is melted, it wraps the suspended heat source. Since the conductive property of the suspended heat source is good, the suspended melt can be kept suspended in the alternating magnetic field. Furthermore, after the suspended melt is formed, the weight of the suspended melt is greater than the weight of the suspended heat source 5. Therefore, if the suspended state of the suspended melt is to be kept unchanged, the frequency or power of the induction coil should be adjusted in theory to appropriately increase the upward second electromagnetic force.

[0074] As described in the above embodiments, the present application does not limit the shape of the suspended heat source, and the shape of the suspended heat source includes but is not limited to an inverted cone, a sphere, or a cylinder, etc., as long as it can be stably suspended and melt the gallium oxide rod material. In addition, the present application does not limit the weight of the suspended heat source, as long as a suspended heat source of appropriate weight is selected according to the size of the gallium oxide single crystal to be grown. If a gallium oxide single crystal with a diameter of more than 2 inches is to be grown, the weight m of the suspended heat source in this embodiment is preferably within 1g-100g.

[0075] In this embodiment, the diameter of the side of the suspended heat source 5 in contact with the gallium oxide material rod is D1, the diameter of the gallium oxide material rod is D2, and the diameter of the grown gallium oxide single crystal is D3. In order to facilitate faster melting of the gallium oxide material rod, D1≥D2, and the diameter of the grown gallium oxide single crystal is D3≥D2.

[0076] In this embodiment, the shape of the suspended heat source is an inverted cone as an example. The bottom diameter of the suspended heat source is D1, the weight is m, and the density is ρ, wherein D1=(24m×tanβ / (πρ))^(1 / 3).

[0077] Step S16: stop introducing the first flowing gas, start introducing the second flowing gas, and form a stable flowing atmosphere.

[0078] The function of the first flowing gas is to protect the suspended heat source from being oxidized during the process of heating and melting the suspended heat source material. Therefore, the first flowing gas is preferably an inert gas, and more preferably, the first flowing gas is argon or nitrogen.

[0079] The function of the first flowing gas is to make the gallium oxide single crystal grow smoothly and inhibit the decomposition and volatilization of the gallium oxide melt. The growth process of the gallium oxide single crystal needs to be in an atmosphere containing oxygen. The higher the oxygen concentration, the smoother the growth process of the gallium oxide single crystal. Therefore, in this embodiment, the second flowing gas includes a mixed gas of oxygen and other gases, and the other gases include one or more of carbon dioxide, argon, and nitrogen. The oxygen content in the second flowing gas accounts for X, 0<X≤100%.

[0080] It should be noted that there are many ways to dope gallium oxide single crystals, and the doping methods in the process of gallium oxide single crystal growth include but are not limited to solid-state doping and gas-phase doping. The so-called solid-state doping is to add doping elements to the raw materials, and then introduce the doping elements into the crystal through the crystal growth process. Gas-phase doping is to introduce doping elements through a gas source during the crystal growth process.

[0081] If the gallium oxide single crystal is grown by solid-state doping, the doping conditions of the gallium oxide material rod 21 and the gallium oxide seed crystal 31 match the electrical type of the gallium oxide single crystal to be grown. When the electrical type of the gallium oxide single crystal to be grown is n-type, the doping elements of the gallium oxide material rod 21 and the gallium oxide seed crystal 31 can be donor impurities such as selenium (Se), tin (Sn), and indium (In); when the electrical type of the gallium oxide single crystal to be grown is p-type, the doping elements of the gallium oxide material rod 21 and the gallium oxide seed crystal 31 can be acceptor impurities such as boron (B), magnesium (Mg), zinc (Zn), and aluminum (Al); when the electrical type of the gallium oxide single crystal to be grown is unintentional doping, the gallium oxide material rod 21 and the gallium oxide seed crystal 31 are not doped with other elements.

[0082] If the gallium oxide single crystal is grown by gas phase doping, the second flowing gas contains doping elements that match the electrical type of the gallium oxide single crystal to be grown. When the electrical type of the gallium oxide single crystal to be grown is n-type, the doping elements of the second flowing gas can be donor impurities such as selenium (Se), tin (Sn), and indium (In); when the electrical type of the gallium oxide single crystal to be grown is p-type, the doping elements of the second flowing gas can be acceptor impurities such as boron (B), magnesium (Mg), zinc (Zn), and aluminum (Al); when the electrical type of the gallium oxide single crystal to be grown is unintentionally doped, the second flowing gas is not doped with other elements.

[0083] Step S17: Entering the crystal growth stage: raising the lower seed crystal rod 3 so that the top of the gallium oxide seed crystal 31 is close to and contacts the bottom of the suspended melt, that is, the top of the gallium oxide seed crystal 31 contacts the suspended melt zone 22 of the outer layer of the suspended melt, adjusting the descending rate of the lower seed crystal rod so that the gallium oxide single crystal starts to grow along the top of the gallium oxide seed crystal until the grown gallium oxide single crystal reaches the target size, continuing to descend the lower seed crystal rod so that the generated gallium oxide crystal is separated from the suspended melt, and then the upper seed crystal rod stops descending.

[0084] During the growth of the gallium oxide single crystal, the upper seed crystal rod 2 is continuously lowered to continuously melt the gallium oxide material rod and maintain the state of the suspended melt, and the second flowing gas is continuously introduced into the furnace drum 11 .

[0085] like Figure 4 As shown, after entering the crystal growth stage, the molten gallium oxide rod material gradually forms a molten pool 23 under the suspended melt, and the material at the bottom of the molten pool 23 is cooled under the guidance of the seed crystal to form a single crystal consistent with the seed crystal.

[0086] The crystal growth stage is based on growing a gallium oxide single crystal of a target size. The specific growth process can be adjusted according to the shape of the target gallium oxide single crystal and other requirements, which is not limited in this embodiment.

[0087] Step S18: Entering the furnace shutdown stage: maintaining the suspended melt state and continuing to suspend, stopping the introduction of the second flowing gas, and starting the introduction of the first flowing gas, until the molten gallium oxide rod material (i.e., the suspended melt zone) wrapping the suspended heat source in the suspended melt is volatilized and decomposed, stopping the introduction of the first flowing gas, starting the introduction of the second flowing gas, and gradually reducing the power of the induction coil to zero, so that the suspended heat source is oxidized and cooled to form a solid block and falls; when the furnace drum temperature drops to the target temperature, stopping the introduction of the second flowing gas.

[0088] Gallium oxide has the characteristics of being easy to decompose and volatilize in the molten state, and the conditions for its volatilization must meet: maintaining the molten state and reducing the oxygen content in the atmosphere. Therefore, in this embodiment, the characteristics of gallium oxide being easy to decompose and volatilize in the molten state are utilized to keep the frequency and power of the induction coil unchanged, so as to keep the suspended melt zone of the outer layer of the suspended melt in the molten state at all times, and stop introducing the second flowing gas containing oxygen and instead introduce an inert gas, which can facilitate the volatilization of the suspended melt zone in an oxygen-free atmosphere on the one hand, and protect the suspended heat source on the other hand, so as to avoid the suspended heat source being oxidized during the volatilization of the suspended melt zone, thereby causing the unstable suspended state to occur.

[0089] When the suspended molten zone volatilizes and decomposes, the inert gas is stopped and replaced by a second flowing gas containing oxygen, taking advantage of the fact that the suspended heat source is easily oxidized and its conductivity is reduced after oxidation. This allows the suspended heat source to oxidize and cool down to form a solid block that falls onto the gallium oxide single crystal or the lower cover. The power of the induction coil is then reduced to 0. When the temperature in the furnace barrel drops to room temperature, the gas is stopped, and the furnace is opened to take out the gallium oxide single crystal and the oxidized suspended heat source.

[0090] It should be noted that in each stage of steps S12-S18, the present application does not specifically limit the flow rate of the first flowing gas or the second flowing gas introduced in each stage. The flow rate of the gas can be adaptively adjusted according to the growth rate of the gallium oxide single crystal and the temperature and pressure in the furnace. In theory, the larger the size of the growing gallium oxide single crystal and the larger the diameter of the furnace, the greater the required gas flow rate. In order to maintain the gas flow stability during the crystal growth process, the gas flow rate of each stage of the embodiment of the present application is preferably kept unchanged, and the gas flow rate is preferably within 0.1L / min-100L / min.

[0091] Furthermore, during the entire process of steps S12-S18, since impurities are easily deposited at the gas outlet channel, in order to prevent the impurities in the gas outlet channel from being blown back into the furnace and causing contamination of the gallium oxide single crystal, the gas flow direction must be kept consistent throughout the entire process and cannot be easily changed.

[0092] In the entire growth process of the embodiment of the present application, no precious metal materials such as iridium are involved. Only a spiral induction coil wound around the periphery of the furnace drum provides a high-frequency alternating magnetic field when energized. The downward first electromagnetic force generated by the stabilizing coil in the induction coil and the upward second electromagnetic force generated by the suspension heating coil interact with each other, so that the suspended heat source material fed into the furnace drum through the feeding channel above the furnace drum can be stably suspended in the working area surrounded by the induction coil in the working state, and the suspension heating coil can also heat the suspended heat source material to melt the suspended heat source material to obtain a suspended heat source, and keep the suspended heat source in a molten working state during the entire crystal growth process.

[0093] Later, during the crystal growth process, the suspended heat source in a molten state is used as a heat source to contact the gallium oxide material rod installed on the upper seed crystal rod, and the gallium oxide material rod is heated so that the gallium oxide material rod is melted by the heat and completely wraps the suspended heat source to form a suspended melt, that is, the core of the suspended melt is the suspended heat source in a molten state, and the outer layer is the molten gallium oxide material rod material. After obtaining the suspended melt, the upper seed crystal rod is continuously lowered to allow the material rod to continue to melt, and at the same time, the lower seed crystal rod is raised to allow the gallium oxide seed crystal to contact the suspended melt, and the crystal growth process is started until the gallium oxide single crystal of the target size is obtained, and then the furnace shutdown stage is entered. Since the molten gallium oxide material rod material is easy to volatilize in an oxygen-deficient atmosphere, the present application first creates an oxygen-deficient atmosphere in the furnace drum to volatilize the molten gallium oxide material rod material on the outer layer of the suspended melt, and since the suspended heat source material can be oxidized to form an oxide solid in an oxidizing atmosphere, the oxide has poor conductivity, and the electromagnetic suspension force it is subjected to becomes smaller, so that it can gradually fall to the bottom of the furnace drum for removal.

[0094] A flow chart of a gallium oxide single crystal growth method disclosed in another embodiment of the present application is as follows: Figure 3 As shown, Figure 2 The method shown is different in that the specific process of the crystal growth stage is further clarified. Specifically, the crystal growth stage includes the seeding stage, necking stage, shoulder release stage, equal diameter stage, and finishing stage of step S27-step S31. The process of steps S21-S26 and S32 in this embodiment is similar to the process of steps S11-step S16 and S18 in the previous embodiment, and will not be repeated here. Specifically, the process of each stage of the crystal growth stage in this embodiment is: Step S27: seeding stage: the lower seed crystal rod 3 rises at a second rate V2, so that the top of the gallium oxide seed crystal 31 approaches and contacts the bottom of the suspended melt, that is, the top of the gallium oxide seed crystal 31 approaches and contacts the bottom of the suspended melt zone 22 of the outer layer of the suspended melt, so that the gallium oxide material in the molten state of the suspended melt zone gradually solidifies and grows into a gallium oxide single crystal consistent with the seed crystal under the seeding action of the seed crystal.

[0095] The seeding process can be divided into a process of preheating the seed crystal and a process after preheating. In the preheating process, the lower seed crystal rod 3 can be slowly raised to make the top of the gallium oxide seed crystal 31 close to but not in contact with the bottom of the suspension melt 22, and the lower seed crystal rod 3 is stopped from being raised and stays at this position for a certain period of time, so that the seed crystal can be preheated under the influence of the heat of the suspension melt 22; after the preheating is completed, the lower seed crystal rod 3 is continued to be raised to make the top of the gallium oxide seed crystal 31 contact with the bottom of the suspension melt 22.

[0096] In this embodiment, the specific value of V2 is not limited and can be adjusted according to actual conditions to ensure that the state of the gallium oxide seed crystal is controllable.

[0097] Step S28: Neck shrinkage stage: the lower seed crystal rod 3 descends at a third rate V3, so that the gallium oxide single crystal begins to grow along the top of the gallium oxide seed crystal 31 and forms a thin neck. During this process, the upper seed crystal rod 2 continues to descend to keep the gallium oxide material rod melted and maintain the state of the suspended melt. As above, the specific value of V3 is not limited in this embodiment and can be adjusted according to actual conditions to ensure that the state of the crystal growth process is controllable.

[0098] In this process, the lower seed crystal rod 3 descends, providing a certain growth time and cooling time for the growth of the gallium oxide single crystal. In this process, the power and frequency of the induction coil remain unchanged.

[0099] Step S29: shoulder release stage: the lower seed crystal rod 3 descends at a fourth rate V4, and / or the power of the induction coil 4 is reduced to expand the diameter of the grown gallium oxide single crystal. During this process, the upper seed crystal rod continues to descend to melt the gallium oxide material rod and maintain the state of the suspended melt, wherein V4 < V3. During the crystal growth process, the gallium oxide material rod material still in a molten state gathers under the suspended melt to form a molten pool 23, and the diameter of the molten pool 23 directly affects the diameter of the gallium oxide single crystal.

[0100] In the crystal growth stage, the descending speed of the lower seed crystal rod 3 is reduced, and on the basis of keeping the melting rate of the gallium oxide material rod basically unchanged, the diameter and volume of the molten pool 23 can be increased, thereby increasing the diameter of the gallium oxide single crystal. In addition, reducing the power of the induction coil 4 will reduce the temperature in the furnace drum, especially in the suspended melt area and the molten pool area in contact with the suspended melt. When the descending speed of the lower seed crystal rod 3 remains unchanged, the temperature in the furnace drum is reduced, which will accelerate crystallization, thereby causing the diameter of the gallium oxide single crystal to grow longer and larger.

[0101] In this embodiment, the descending speed of the lower seed crystal rod 3 can be reduced alone, or the power of the induction coil 4 can be reduced alone. Alternatively, the descending speed of the lower seed crystal rod 3 can be reduced, or the power of the induction coil 4 can be reduced at the same time. This embodiment does not limit this.

[0102] Step S30: equal diameter stage: when the diameter of the grown gallium oxide single crystal is expanded to the target size, the lower seed crystal rod 3 descends at a fifth rate V5 to maintain the diameter of the grown gallium oxide single crystal at the target size. During this process, the upper seed crystal rod continues to descend to melt the gallium oxide material rod and maintain the state of the suspended melt, wherein V5<V4.

[0103] In the equal diameter stage, the diameter of the gallium oxide single crystal has been expanded to the target size. It is only necessary to maintain a stable descending rate of the lower seed crystal rod 3 or maintain the power of the induction coil to keep the diameter of the molten pool 23 at the target size, so that the diameter of the grown gallium oxide single crystal can be maintained at the target size. In the equal diameter stage, in this embodiment, it is preferred that the descending rate of the lower seed crystal rod (i.e., the growth rate of the gallium oxide single crystal) V5 is within 0.5 mm / h-50 mm / h.

[0104] Step S31: Finishing stage: when the length of the grown gallium oxide single crystal reaches the target size, the lower seed crystal rod 3 descends at a sixth rate V6, and / or the power of the induction coil is increased, so that the diameter of the grown gallium oxide single crystal gradually decreases until it is separated from the suspended melt. When the gallium oxide single crystal is separated from the suspended melt, the upper seed crystal rod stops descending, wherein V6>V5.

[0105] It should be noted that, compared with the equal diameter stage, in the final stage, the lower seed crystal rod 3 is increased in descending speed, and on the basis of keeping the melting rate of the gallium oxide material rod basically unchanged, the diameter and volume of the molten pool 23 can be reduced, thereby reducing the diameter of the gallium oxide single crystal. In addition to increasing the descending speed of the lower seed crystal rod 3, the power of the induction coil 4 can also be increased. Increasing the power of the induction coil 4 will increase the temperature in the furnace drum, especially in the suspended melt area and the molten pool area in contact with the suspended melt. When the descending speed of the lower seed crystal rod 3 remains unchanged, the temperature in the furnace drum will increase, which will inhibit crystallization, reduce the crystallization rate, and thereby reduce the diameter of the gallium oxide single crystal.

[0106] Of course, in this process, in this embodiment, the descending speed of the lower seed crystal rod 3 can be increased alone, or the power of the induction coil 4 can be increased alone. It is also possible to increase the descending speed of the lower seed crystal rod 3 and the power of the induction coil 4 at the same time. This is not limited in this embodiment, as long as the diameter of the gallium oxide single crystal can be reduced.

[0107] In the entire crystal growth stage in this embodiment, similar to the previous embodiment, the flow rate of the first flowing gas is equal to the flow rate of the second flowing gas. In the entire crystal growth process, the volume of the suspended melt can be increased or kept unchanged, as long as it can be kept stably suspended in the furnace tube and the suspended melt zone 22 can completely wrap the suspended heat source to prevent the suspended heat source from contacting the second flowing gas containing oxygen.

[0108] It should be noted that during the entire crystal growth stage, the size and rate of the crystal growth can be controlled by controlling the rising or falling rate of the upper seed crystal rod 2 and the lower seed crystal rod 3, or by controlling the power of the induction coil. The rates of the upper seed crystal rod 2 and the lower seed crystal rod 3 and the power of the induction coil can also be flexibly adjusted at the same time. As long as the growth requirements of the single crystal can be met, this embodiment does not limit the specific rate or power adjustment method.

[0109] By using the method disclosed in the embodiment of the present application, the diameter of the gallium oxide single crystal that can be grown is within 2 inches to 8 inches. It can be understood that, in theory, the method disclosed in the embodiment of the present application can be used to grow a larger size of gallium oxide single crystal. The larger the size of the grown gallium oxide single crystal, the larger the size of the required suspension heat source, which requires a larger heating power and suspension force, that is, it is necessary to provide a larger power to the induction coil. However, the power that the induction coil can withstand is limited. Exceeding the limit will cause the induction coil to be destroyed. Therefore, the size of the grown gallium oxide single crystal is also limited. Of course, by adjusting the material of the induction coil or the cooling efficiency of the coolant, it is also possible to moderately increase the size of the gallium oxide single crystal.

[0110] The following takes the growth of a 2-inch unintentionally doped gallium oxide single crystal as an example to illustrate the gallium oxide single crystal growth method disclosed in the embodiment of the present application.

[0111] Step 1: Assemble the gallium oxide single crystal growth device, install the gallium oxide material rod on the upper seed crystal rod, install the gallium oxide seed crystal on the lower seed crystal rod, and then close the upper cover and the lower cover to form a closed space in the furnace.

[0112] The furnace tube can be a quartz tube, and a suspended heat source material is prepared. The suspended heat source material in this embodiment is preferably metal Ga, and the weight can be 5g. The number of turns of the stabilizing coil is N1≤10, the number of turns of the heating coil is N2≤20, and the number of turns of the suspension coil is N3≤20. Taking the induction coil with 7 turns as an example, N1=1, N2=4, N3=2, and the vertical spacing of the turns is d1=d2=d3=1mm. The diameter of the stabilizing coil and the heating coil can be 80mm-100mm, preferably 90mm. The diameter of the suspension coil can be equal to the diameter of the heating coil, or it can be an inverted cone. If it is an inverted cone, the semi-cone angle of the suspension coil is 10°<β≤30°, preferably, β=18.5°, and the diameter of the suspension coil can be between 80mm-90mm. If the outer diameter of the quartz tube is 80mm, the minimum diameter of the suspension coil can be 82mm, leaving space for the thermal expansion of the quartz tube and the flow of gas.

[0113] Step 2: Open the lower cover air inlet channel and the upper cover air outlet channel of the closed furnace tube, and introduce the first flowing gas from top to bottom to form a stable flowing atmosphere. The first flowing gas is preferably argon.

[0114] Step 3, the feeding stage, which can also be called the suspended heat source preheating stage, sets the induction coil frequency to 100kHz, and at the same time, the power is quickly increased to 20kW, and then the suspended heat source material is fed from the feeding port into the inner area of ​​the furnace drum within the induction coil through the feeding channel, so that the suspended heat source material melts to form an inverted cone shape and is stably suspended, and then the area surrounded by the induction coil is heated to the melting point of the gallium oxide rod, such as 1800°C.

[0115] Step 4, feeding stage. The upper seed crystal rod descends to gradually bring the bottom of the material rod close to the suspension heat source, the material rod is heated and melted, and the molten material of the material rod is wrapped outside the suspension heat source. Continue to feed slowly to increase the volume of the suspension melting zone until the suspension heat source is completely wrapped to obtain a suspension melt.

[0116] Step 5: Stop introducing argon gas into the furnace tube and introduce the second flowing gas instead to form a stable flowing atmosphere. The second flowing gas may be a mixed gas of 20% oxygen + 80% carbon dioxide.

[0117] Step 6, seeding stage: The lower seed crystal rod rises to make the top of the seed crystal close to the bottom of the suspended heat source for preheating; after preheating for about 20 minutes, the lower seed crystal rod continues to rise slowly to make the top of the seed crystal contact with the bottom of the suspended melt.

[0118] Step 7, necking stage. The lower seed crystal rod then descends at a speed of 20 mm / h, causing the crystal to grow along the top of the seed crystal and form a thin neck. During this process, the upper seed crystal rod continues to descend to melt the material rod to maintain the volume of the suspended melt unchanged.

[0119] Step 8, shoulder release stage. Reduce the descending rate of the lower seed crystal rod to 5 mm / h to expand the diameter of the gallium oxide single crystal. During this process, the upper seed crystal rod is continuously lowered to melt the material rod to maintain the volume of the suspended melt unchanged.

[0120] Step 9, equal diameter stage. When the crystal diameter is expanded to 2 inches, the descending rate of the lower seed crystal rod is increased to 10 mm / h, so that the diameter of the gallium oxide single crystal remains unchanged and the length gradually increases. During this process, the upper seed crystal rod is continuously descended to melt the material rod to maintain the volume of the suspended melt unchanged.

[0121] Step 10, final stage. Increase the descending rate of the lower seed crystal rod to 20 mm / h, so that the diameter of the gallium oxide single crystal gradually decreases until it is separated from the melt. When the crystal is separated from the melt, the upper seed crystal rod stops descending.

[0122] Step 11, furnace shutdown stage. Keep the frequency and power of the induction coil unchanged, keep the suspended melt suspended, introduce argon gas, and completely volatilize and decompose the molten gallium oxide material in the suspended melt zone, exposing the suspended heat source; then introduce the second flowing gas, the suspended heat source gradually oxidizes to form an oxide solid, cools down and solidifies, and then lands on the gallium oxide crystal or the lower cover. Then slowly reduce the power of the induction coil to 0, and when the temperature in the furnace barrel drops to room temperature, stop introducing gas and open the furnace to take out the grown gallium oxide single crystal.

[0123] In the description of the present invention, it is to be understood that the terms “center”, “longitudinal”, “lateral”, “length”, “width”, “thickness”, “up”, “down”, “front”, “back”, “left”, “right”, “vertical”, “horizontal”, “top”, “bottom”, “inside”, “outside”, “clockwise”, “counterclockwise”, “axial”, “radial”, “circumferential”, etc., indicating orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0124] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0125] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0126] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0127] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "upper", "lower", "left", "right" and similar expressions used herein are for illustrative purposes only and do not represent the only implementation method.

[0128] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0129] It should be understood that, although the various steps in the flowcharts involved in the above-mentioned embodiments are displayed in sequence according to the indication of the arrows, these steps are not necessarily executed in sequence according to the order indicated by the arrows. Unless there is a clear explanation in this article, the execution of these steps is not strictly limited in order, and these steps can be executed in other orders. Moreover, at least a part of the steps in the flowcharts involved in the above-mentioned embodiments can include multiple steps or multiple stages, and these steps or stages are not necessarily executed at the same time, but can be executed at different times, and the execution order of these steps or stages is not necessarily carried out in sequence, but can be executed in turn or alternately with other steps or at least a part of the steps or stages in other steps.

[0130] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0131] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.

Claims

1. A gallium oxide single crystal growth device, It is characterized in that include: A furnace body, the furnace body comprising a furnace barrel, an upper cover and a lower cover respectively arranged at both ends of the furnace barrel, the upper cover being provided with a feeding channel and a first gas channel communicating with the interior of the furnace barrel, the feeding channel being used to feed suspended heat source materials into the furnace barrel, and the lower cover being provided with a second gas channel communicating with the interior of the furnace barrel; An upper seed crystal rod passing through the upper cover, the upper seed crystal rod being used to place a gallium oxide material rod; A lower seed crystal rod passing through the lower cover, wherein the lower seed crystal rod is used to place gallium oxide seed crystals; The spiral induction coil wound around the outer periphery of the furnace drum is used to provide a high-frequency alternating magnetic field; the induction coil includes a stabilizing coil and a suspension heating coil from top to bottom, the stabilizing coil generates a first downward electromagnetic force when energized, and the suspension heating coil generates a second upward electromagnetic force when energized, the first electromagnetic force and the second electromagnetic force interact with each other so that the suspension heat source placed in the furnace drum is stably suspended in the working area surrounded by the induction coil in the working state.

2. The gallium oxide single crystal growth device according to claim 1, It is characterized in that The winding direction of the stabilizing coil is opposite to the winding direction of the suspension heating coil; And / or, the metal pipeline around which the induction coil is wound is a hollow structure, and the metal pipeline around which the stabilization coil is wound is connected to the metal pipeline around which the suspension heating coil is wound; And / or, the first gas channel is an air outlet channel, and the second gas channel is an air inlet channel.

3. The gallium oxide single crystal growth device according to claim 1, It is characterized in that The suspension heating coil comprises a heating coil and a suspension coil from top to bottom, the heating coil is wound in a cylindrical shape, the suspension coil is wound in an inverted cone shape, and the setting range of the semi-cone angle β of the suspension coil is 0°<β≤90°; And / or, the number of turns of the stabilizing coil is N1, the number of turns of the heating coil is N2, and the number of turns of the suspension coil is N3, wherein N1≤N2, and N1≤N3; And / or, the vertical spacing between the turns of the stabilizing coil is d1, the vertical spacing between the turns of the heating coil is d2, and the vertical spacing between the turns of the suspension coil is d3, wherein d1≥d2, and d1≥d3.

4. The gallium oxide single crystal growth device according to any one of claims 1 to 3, It is characterized in that The furnace tube is a sapphire tube or a quartz tube; And / or, the diameter of the gallium oxide single crystal grown by the gallium oxide single crystal growth device is D, and the inner diameter of the furnace drum is within a range of 1.2D-3D.

5. A method for growing a gallium oxide single crystal, It is characterized in that Using the gallium oxide single crystal growth device according to any one of claims 1 to 4, the growth method comprises: Installing a gallium oxide material rod on the upper seed crystal rod, and installing a gallium oxide seed crystal on the lower seed crystal rod; A first flowing gas is introduced into the furnace barrel through the first gas channel and the second gas channel to form a stable flowing atmosphere in the furnace barrel; An alternating current of a preset frequency and a preset magnitude is passed through the induction coil to form a high-frequency alternating magnetic field of a target frequency and a target power in a working area enclosed by the induction coil in the furnace drum; A suspended heat source material is fed into the furnace drum through the feeding channel. Under the action of the high-frequency alternating magnetic field, the stabilizing coil generates a first downward electromagnetic force after being energized, and the suspended heating coil generates a second upward electromagnetic force after being energized. The first electromagnetic force and the second electromagnetic force interact with each other to melt the suspended heat source material in the working area to obtain a suspended heat source, and the suspended heat source is stably suspended in the working area, wherein the working temperature of the suspended heat source is T1, the melting point of the gallium oxide material rod is T2, T1>T2, the suspended heat source material has good electrical conductivity, a boiling point higher than the melting point of the gallium oxide material rod, the suspended heat source material has low reactivity or low solid solubility limit with the molten gallium oxide material rod material, and does not change the electrical type of the gallium oxide single crystal in the molten state; Entering the feeding stage: the upper seed crystal rod descends at a first speed V1, so that the bottom end of the gallium oxide material rod approaches and contacts the suspended heat source, so that the gallium oxide material rod is heated and melted, and the upper seed crystal rod is continuously descended until the molten gallium oxide material rod completely wraps the suspended heat source to form a suspended melt, and the suspended melt remains suspended under the action of the high-frequency alternating magnetic field; Stop introducing the first flowing gas, start introducing the second flowing gas, and form a stable flowing atmosphere; Entering the crystal growth stage: raising the lower seed crystal rod so that the top of the gallium oxide seed crystal approaches and contacts the bottom of the suspended melt, adjusting the descending rate of the lower seed crystal rod so that the gallium oxide single crystal starts to grow along the top of the gallium oxide seed crystal until the grown gallium oxide single crystal reaches a target size, continuing to descend the lower seed crystal rod so that the generated gallium oxide crystal is separated from the suspended melt, and then the upper seed crystal rod stops descending; during the growth of the gallium oxide single crystal, the upper seed crystal rod continues to descend so that the gallium oxide material rod continues to melt and maintain the state of the suspended melt, and the second flowing gas continues to flow into the furnace barrel; Entering the shutdown stage: maintaining the suspended melt state and continuing to suspend, stopping the introduction of the second flowing gas, and starting the introduction of the first flowing gas, until the molten gallium oxide rod material wrapping the suspended heat source in the suspended melt is volatilized and decomposed, stopping the introduction of the first flowing gas, starting the introduction of the second flowing gas, and gradually reducing the power of the induction coil to zero, so that the suspended heat source is oxidized and cooled to form a solid block and fall; when the furnace drum temperature drops to the target temperature, stopping the introduction of the second flowing gas.

6. The gallium oxide single crystal growth method according to claim 5, It is characterized in that The crystal growth stages include seeding stage, necking stage, shoulder release stage, equal diameter stage, and finishing stage. The process of each stage is as follows: Seeding stage: the lower seed crystal rod rises at a second rate V2, so that the top of the gallium oxide seed crystal approaches and contacts the bottom of the suspended melt; Neck shrinking stage: the lower seed crystal rod descends at a third rate V3, so that the gallium oxide single crystal begins to grow along the top of the gallium oxide seed crystal and forms a thin neck. During this process, the upper seed crystal rod continues to descend to melt the gallium oxide material rod and maintain the state of the suspended melt; Shoulder release stage: the lower seed crystal rod descends at a fourth rate V4, and / or the power of the induction coil is reduced to expand the diameter of the grown gallium oxide single crystal. During this process, the upper seed crystal rod continues to descend to melt the gallium oxide material rod and maintain the state of the suspended melt, wherein V4<V3; Equal diameter stage: when the diameter of the grown gallium oxide single crystal is expanded to the target size, the lower seed crystal rod descends at a fifth rate V5 to maintain the diameter of the grown gallium oxide single crystal at the target size. During this process, the upper seed crystal rod continues to descend to melt the gallium oxide material rod and maintain the state of the suspended melt, wherein V5<V4; Finishing stage: when the length of the grown gallium oxide single crystal reaches the target size, the lower seed crystal rod descends at a sixth rate V6, and / or the power of the induction coil is increased, so that the diameter of the grown gallium oxide single crystal gradually decreases until it is separated from the suspended melt. When the gallium oxide single crystal is separated from the suspended melt, the upper seed crystal rod stops descending, wherein V6>V5.

7. The gallium oxide single crystal growth method according to claim 5, It is characterized in that The first flowing gas is an inert gas, the second flowing gas is a mixed gas containing oxygen and other gases, the other gases include one or more of carbon dioxide, argon, and nitrogen, and the oxygen content in the second flowing gas is X, 0<X≤100%; And / or, the flow rate of the first flowing gas is equal to the flow rate of the second flowing gas.

8. The gallium oxide single crystal growth method according to claim 5, It is characterized in that When the electrical type of the gallium oxide single crystal is n-type, the suspended heat source material is Sn, Si, Ta or Nb; when the electrical type of the gallium oxide single crystal is semi-insulating, the suspended heat source material is Fe or Mg; when the electrical type of the gallium oxide single crystal is unintentionally doped, the suspended heat source material is Ga; and / or, the operating temperature T1 of the suspension heat source is within the range of 1750°C-1900°C; And / or, the weight m of the suspended heat source is within 1g-100g.

9. The gallium oxide single crystal growth method according to claim 5, It is characterized in that The diameter of the side of the suspended heat source in contact with the gallium oxide material rod is D1, the diameter of the gallium oxide material rod is D2, and the diameter of the gallium oxide single crystal is D3, wherein D1≥D2, and D3≥D2; And / or, the shape of the suspended heat source is an inverted cone, a sphere, or a cylinder. When the shape of the suspended heat source is an inverted cone, the bottom diameter of the suspended heat source is D1, the weight is m, the density is ρ, Where, D1=(24m×tanβ / (πρ))^(1 / 3); And / or, the diameter of the gallium oxide single crystal is within 2 inches to 8 inches.

10. The gallium oxide single crystal growth method according to claim 6, It is characterized in that During operation, the frequency of the induction coil is within 1 kHz-500 kHz, the power of the induction coil is within 1 kW-2000 kW, and the frequency of the induction coil remains unchanged during operation; And / or, in the equal diameter stage, the descending rate V5 of the lower seed rod is within 0.5 mm / h-50 mm / h.

Citation Information

Patent Citations

  • Method and device for growing flaky gallium oxide crystals by micro pull-down zone melting method

    CN115142130A

  • Gallium oxide crystal growth device and crystal growth method

    CN116219546A

  • Device for growing gallium oxide crystal by induction zone melting method

    CN116791188A

  • Magnetic suspension melting apparatus

    EP0641146A1

  • Device and method for levitation melting using induction units which are arranged in a tilted manner

    IN202017028712A