Regenerated cellulose fiber as well as preparation method and application thereof
Through the mixing and spinning process of functionalized graphene and cellulose in ionic liquid, the problem of insufficient breaking strength and elongation of regenerated cellulose fibers in the prior art is solved, and the preparation of high-performance regenerated cellulose fibers is realized. In high-end textiles.
Patent Information
- Application Number
- CN202410990973.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-23
AI Technical Summary
The existing methods for preparing regenerated cellulose fibers are difficult to take into account the break strength and elongation of break, and the preparation process is complex and costly, which affects its application in high-end textiles.
Functionalized graphene and initial cellulose are mixed in an ionic liquid to form a cellulose spinning liquid, and regenerated cellulose fibers are prepared through spinning process without adding dispersant to avoid pre-melting and high-temperature treatment.
The obtained regenerated cellulose fibers have high break strength and elongation of break, with break strength up to 2.75cN/dtex and elongation of break of more than 8.10%. The process is simple and the cost is low.
Smart Images

Figure CN118932514A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a regenerated cellulose fiber and a preparation method and application thereof. Background Art
[0002] Regenerated cellulose fiber has gradually become an important direction for the green transformation of the textile industry due to its advantages such as wide sources, renewability, biodegradability and good biocompatibility.
[0003] Regenerated cellulose fiber has broad application prospects in many fields such as textiles, medical care, and construction. However, the current preparation methods of regenerated cellulose fiber generally have problems such as the inability to balance strength and elongation at break, complex preparation process, and high cost, which limit its application in large-scale industrial production.
[0004] Traditional regenerated cellulose fiber preparation methods, such as the viscose method, can achieve cellulose regeneration, but they release a large amount of toxic gases during the production process, which not only harms human health but also seriously pollutes the environment. In addition, the strength and elongation at break of the regenerated cellulose fiber obtained by this method are both low, which cannot meet the material performance requirements of high-end textiles.
[0005] CN116590801A discloses a method for preparing regenerated cellulose fiber by using a composite coagulation bath, comprising: adding cellulose to an ionic liquid for swelling; heating and dissolving the swollen raw material, and degassing under vacuum conditions to obtain a spinning solution; using a single solvent or a mixed solution of multiple solvents as a coagulation bath, and regenerating the spinning solution in the coagulation bath by dry-jet wet spinning to obtain regenerated cellulose fiber. The breaking strength and breaking elongation of the regenerated cellulose fiber obtained by this method need to be further improved.
[0006] CN106149083A discloses a functional graphene cellulose fiber prepared by a melting method and a preparation method thereof, the preparation method comprising: preparing a graphene dispersion, preparing a cellulose / ionic liquid mixture, mixing, pre-melting, preparing a spinning solution and spinning steps. The cellulose fiber obtained by the preparation method has a high breaking strength, but the preparation method requires pre-melting and the addition of a dispersant, and the preparation process is relatively complicated.
[0007] CN109183170A discloses a method for preparing cellulose graphene composite staple fibers, comprising: mixing a dispersant, graphene oxide and cellulose and dissolving them in an ionic liquid aqueous solution, wherein the addition amount of graphene oxide is 0.1-0.3wt% of the cellulose to obtain a mixed spinning solution; the obtained mixed spinning solution is filtered, spun, coagulated, stretched, washed, bleached, oiled, cut, and dried to obtain cellulose graphene composite staple fibers. The breaking strength of the composite staple fibers obtained by the preparation method is acceptable, but the breaking elongation still needs to be improved, and a dispersant needs to be added in the preparation method. CN109267164A discloses a method for preparing cellulose graphene composite filaments, the breaking strength of the composite filaments obtained by the preparation method is acceptable, but the breaking elongation still needs to be improved, and a dispersant also needs to be added in the preparation method. Summary of the invention
[0008] In view of this, one object of the present invention is to provide a method for preparing regenerated cellulose fibers, wherein the regenerated cellulose fibers obtained by the preparation method have both high breaking strength and breaking elongation. Another object of the present invention is to provide a regenerated cellulose fiber obtained according to the preparation method as described above. Another object of the present invention is to provide an application of the regenerated cellulose fibers as described above.
[0009] The present invention adopts the following technical solutions to achieve the above-mentioned purpose.
[0010] In one aspect, the present invention provides a method for preparing regenerated cellulose fiber, comprising the following steps:
[0011] 1) dispersing the functionalized graphene in an ionic liquid to obtain a functionalized graphene dispersion;
[0012] 2) mixing the initial cellulose with the functionalized graphene dispersion obtained in step 1) to obtain a cellulose spinning solution;
[0013] 3) spinning the cellulose spinning solution obtained in step 2) to obtain regenerated cellulose fibers;
[0014] Wherein, the functionalized graphene is selected from at least one of amino graphene, hydroxylated graphene and fluorinated graphene;
[0015] Wherein, the initial cellulose is selected from wood pulp cellulose and / or cotton pulp cellulose;
[0016] Wherein, the mass ratio of the functionalized graphene to the initial cellulose is 0.05 to 5:100.
[0017] According to the preparation method of the present invention, preferably, in step 1), the mass ratio of the functionalized graphene to the ionic liquid is 0.003-0.015:40-60.
[0018] According to the preparation method of the present invention, preferably, the ionic liquid is an imidazole ionic liquid.
[0019] According to the preparation method of the present invention, preferably, the ionic liquid is selected from one of 1-allyl-3-methylimidazolium chloride, 1-butyl-3-methylimidazolium chloride, 1-ethyl-3-methylimidazolium acetate and 1-ethyl-3-methylimidazolium chloride.
[0020] According to the preparation method of the present invention, preferably, the ionic liquid is 1-allyl-3-methylimidazolium chloride.
[0021] According to the preparation method of the present invention, preferably, the mass ratio of the functionalized graphene to the initial cellulose is 0.1 to 1:100; in step 2), the mixing temperature is 40 to 85°C.
[0022] According to the preparation method of the present invention, preferably, no dispersant is added in step 1) and step 2).
[0023] According to the preparation method of the present invention, preferably, in step 3), the cellulose spinning solution obtained in step 2) is degassed, the degassed cellulose spinning solution is sprayed out through a spinneret, formed in a coagulation bath, and then washed, dried and oiled to obtain regenerated cellulose fibers.
[0024] In another aspect, the present invention further provides a regenerated cellulose fiber, which is prepared according to the preparation method described above.
[0025] In another aspect, the present invention also provides a use of the regenerated cellulose fiber as described above in preparing carbon fiber.
[0026] The regenerated cellulose fiber obtained by the preparation method of the present invention can have both high breaking strength and breaking elongation. Among them, the breaking strength can reach more than 2.75 cN / dtex, and the breaking elongation can reach more than 8.10%. In addition, the preparation method of the present invention does not add any dispersant; no pre-melting is required, and high temperature is not required, and the process is simpler. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the SEM image of the regenerated cellulose fiber obtained in Example 1.
[0028] Figure 2 This is a SEM image of the wood pulp cellulose (i.e., initial cellulose) used in Example 1. DETAILED DESCRIPTION
[0029] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0030] The method for preparing regenerated cellulose fiber of the present invention comprises the following steps: (1) forming a functionalized graphene dispersion solution; (2) forming a cellulose spinning solution; and (3) spinning. The method is described in detail below.
[0031] <Step of Forming Functionalized Graphene Dispersion>
[0032] The functionalized graphene is dispersed in an ionic liquid to obtain a functionalized graphene dispersion. The present invention surprisingly found that the use of functionalized graphene is conducive to the improvement of both the breaking strength and the breaking elongation, and the present invention also found that the functionalized graphene is first dispersed in an ionic liquid to form a dispersion, and then mixed with the initial cellulose, which is more conducive to improving the breaking strength and the breaking elongation. Those skilled in the art know that it is not easy to simultaneously take into account the breaking strength and the breaking elongation.
[0033] In the present invention, the functionalized graphene is selected from at least one of aminated graphene, hydroxylated graphene and fluorinated graphene, preferably selected from one of aminated graphene, hydroxylated graphene and fluorinated graphene, and more preferably selected from one of aminated graphene and hydroxylated graphene. Aminated graphene, hydroxylated graphene and fluorinated graphene are commercially available.
[0034] In the present invention, the mass ratio of the functionalized graphene to the ionic liquid is 0.003-0.015:40-60, preferably 0.003-0.015:50, and more preferably 0.005-0.01:50.
[0035] In the present invention, the ionic liquid is an imidazole ionic liquid. Preferably, the ionic liquid is selected from one of 1-allyl-3-methylimidazolium chloride, 1-butyl-3-methylimidazolium chloride, 1-ethyl-3-methylimidazolium acetate and 1-ethyl-3-methylimidazolium chloride. More preferably, the ionic liquid is 1-allyl-3-methylimidazolium chloride.
[0036] In the present invention, dispersing the functionalized graphene in the ionic liquid specifically comprises the following steps: stirring and mixing the functionalized graphene and the ionic liquid at 40 to 85° C. and 300 to 1000 rpm for 0.5 to 1.5 h, so that the functionalized graphene is uniformly dispersed in the ionic liquid. The temperature during mixing is preferably 50 to 80° C., more preferably 70 to 80° C. The stirring speed is preferably 350 to 800 rpm, more preferably 350 to 500 rpm. The mixing time is preferably 1 to 1.5 h.
[0037] In this step of the present invention, no dispersant is added.
[0038] <Cellulose Spinning Solution Formation Step>
[0039] The initial cellulose is mixed with the obtained functionalized graphene dispersion to obtain a cellulose spinning solution, which is beneficial for improving both the breaking strength and the breaking elongation.
[0040] In the present invention, the initial cellulose may be selected from wood pulp cellulose and / or cotton pulp cellulose. Wood pulp cellulose or cotton pulp cellulose is commercially available. The degree of polymerization of wood pulp cellulose or cotton pulp cellulose may be 200 to 1000, preferably 200 to 800, more preferably 400 to 800, and more preferably 600 to 750.
[0041] In the present invention, the mass ratio of the functionalized graphene to the initial cellulose is 0.05 to 5:100, preferably 0.1 to 1:100, more preferably 0.1 to 0.5:100, more preferably 0.25 to 0.5:100, and further preferably 0.3 to 0.5:100. For example, it can be 0.1:100, 0.15:100, 0.25:100, 0.3:100, 0.35:100, 0.4:100, 0.5:100. The regenerated cellulose fiber obtained in this way can take into account both the breaking strength and the breaking elongation, both of which are relatively high.
[0042] In the present invention, the step of mixing the initial cellulose with the obtained functionalized graphene dispersion specifically includes: stirring and mixing the initial cellulose with the obtained functionalized graphene dispersion at 40-85°C and 300-1000rpm for 1-3h, so that the initial cellulose is fully dissolved in the functionalized graphene dispersion to obtain a cellulose spinning solution. The temperature during mixing can be 40-85°C, preferably 50-80°C, and more preferably 70-80°C. The stirring speed can be 300-1000rpm, preferably 350-850rpm, and more preferably 350-550rpm. The mixing time can be 1-3h, preferably 1-2.5h, and more preferably 1.5-2h.
[0043] In this step of the present invention, no dispersant is added.
[0044] <Spinning Step>
[0045] The obtained cellulose spinning solution is spun to obtain regenerated cellulose fibers, which is conducive to obtaining regenerated cellulose fibers with stable properties.
[0046] In certain specific embodiments, the obtained cellulose spinning solution is degassed, the degassed cellulose spinning solution is ejected through a spinneret, formed in a coagulation bath, and then washed, dried and oiled to obtain regenerated cellulose fibers.
[0047] In the present invention, degassing can be performed under vacuum. The cellulose spinning solution can be delivered to a nozzle 1 to 3 cm away from the coagulation bath by a metering pump. The coagulation bath can be a water bath or an aqueous solution of an ionic liquid. In some embodiments, the coagulation bath is a water bath.
[0048] The drying process can be carried out naturally and the drying temperature can be 25 to 40°C.
[0049] The present invention believes that in the preparation method of the present invention, the ionic liquid and the specific functionalized graphene significantly improve the fluidity of the cellulose spinning solution through synergistic lubrication, laying the foundation for the uniform formation and excellent performance of the regenerated cellulose fiber. At the same time, the amino, hydroxyl or fluoro group in the functionalized graphene can form hydrogen bonds with the hydroxyl group of cellulose, and a strong interaction is formed through the hydrogen bonds, which not only enhances the internal structure of the regenerated cellulose fiber, but also significantly improves the breaking strength and breaking elongation of the regenerated cellulose fiber.
[0050] The present invention also provides a regenerated cellulose fiber prepared according to the preparation method as described above. The fiber has both high breaking strength and breaking elongation. The breaking strength can reach 2.60 cN / dtex or more, preferably 2.75 cN / dtex or more, and more preferably 2.89 cN / dtex or more. The breaking elongation can reach 7.40% or more, preferably 8.10% or more, and more preferably 8.50% or more.
[0051] The regenerated cellulose fiber of the present invention can be used to prepare carbon fiber.
[0052] The test methods used in the following examples are described as follows:
[0053] SEM test: Use scanning electron microscope (SEM500) produced by ZEISS, Germany.
[0054] Breaking strength test: According to (GB / T14337-2008), the tensile speed of the electronic single fiber strength instrument is set to 50mm / min, the return speed is 80mm / min, the initial tension value is 10cN, the clamp distance is 10mm, the experimental temperature is 25℃, and the experimental relative humidity is 40BH%. The fiber to be tested is dried in an oven at 50℃ for 2 hours, and the breaking strength and elongation of the fiber are measured using an electronic single fiber strength instrument.
[0055] The raw materials used in the following examples are described as follows:
[0056] Wood pulp cellulose was provided by Shandong Hailong Co., Ltd., with a degree of polymerization of 702, and was crushed into 49-297 μm by a high-speed pulverizer. 1-Allyl-3-methylimidazolium chloride (CAS: 65039-10-3) was purchased from Beijing Mairida Technology Co., Ltd. Amination of graphene was purchased from Tianjin Ailion Electronic Technology Co., Ltd. Fluorinated graphene was purchased from Tianjin Ailion Electronic Technology Co., Ltd. Hydroxylated graphene was purchased from Anhui Zesheng Technology Co., Ltd.
[0057] Example 1
[0058] The aminated graphene and 1-allyl-3-methylimidazolium chloride ionic liquid were stirred and mixed at 70° C. and 500 rpm for 1 hour, so that the aminated graphene was evenly dispersed in the 1-allyl-3-methylimidazolium chloride ionic liquid to obtain a functionalized graphene dispersion. The mass ratio of the aminated graphene to the 1-allyl-3-methylimidazolium chloride ionic liquid was 0.003:50.
[0059] The wood pulp cellulose (i.e., initial cellulose) and the obtained functionalized graphene dispersion were stirred and mixed at 70° C. and 500 rpm for 1 hour, so that the wood pulp cellulose was fully dissolved in the functionalized graphene dispersion to obtain a cellulose spinning solution, wherein the mass ratio of the amino graphene to the wood pulp cellulose was 0.1:100.
[0060] The cellulose spinning solution is placed in a vacuum drying oven for degassing, and then the degassing cellulose spinning solution is transported to a nozzle 1 to 3 cm away from the coagulation bath by a metering pump. The degassing cellulose spinning solution is ejected from the spinneret and formed in the coagulation bath, and then washed, dried, and oiled to obtain regenerated cellulose fibers. The SEM image of the obtained regenerated cellulose fibers is shown in Figure 1 , the SEM image of wood pulp cellulose (i.e., initial cellulose) is shown in Figure 2 The performance test data of the obtained regenerated cellulose fiber are shown in Table 1.
[0061] Example 2
[0062] Except for the following parameter settings, the rest are the same as Example 1: In this example, the mass ratio of amination graphene to wood pulp cellulose is 0.25:100. The performance test data of the obtained regenerated cellulose fiber is shown in Table 1.
[0063] Example 3
[0064] Except for the following parameter settings, the rest are the same as Example 1: In this example, the mass ratio of amination graphene to wood pulp cellulose is 0.3:100. The performance test data of the obtained regenerated cellulose fiber is shown in Table 1.
[0065] Example 4
[0066] Except for the following parameter settings, the rest are the same as Example 1: In this example, the mass ratio of amination graphene to wood pulp cellulose is 0.4:100. The performance test data of the obtained regenerated cellulose fiber is shown in Table 1.
[0067] Example 5
[0068] Except for the following parameter settings, the rest are the same as Example 1: In this example, the mass ratio of amination graphene to wood pulp cellulose is 0.5:100. The performance test data of the obtained regenerated cellulose fiber is shown in Table 1.
[0069] Table 1
[0070]
[0071] Example 6
[0072] Except for the following parameter settings, the rest is the same as Example 1: the amino graphene is replaced by hydroxylated graphene; the mass ratio of hydroxylated graphene to wood pulp cellulose is 0.2:100. The performance test data of the obtained regenerated cellulose fiber is shown in Table 2.
[0073] Example 7
[0074] Except for the following parameter settings, the rest is the same as Example 1: the amination graphene is replaced by fluorinated graphene; the mass ratio of fluorinated graphene to wood pulp cellulose is 0.2:100. The performance test data of the obtained regenerated cellulose fiber is shown in Table 2.
[0075] Comparative Example 1
[0076] Except for the following parameter settings, the rest is the same as Example 6: hydroxylated graphene is replaced by graphene. The performance test data of the obtained regenerated cellulose fiber is shown in Table 2.
[0077] Table 2
[0078]
[0079] It can be seen from Table 1 and Table 2 that the regenerated cellulose fiber obtained in the present invention has a relatively high breaking strength and a relatively high breaking elongation.
[0080] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.
Claims
1. A method for preparing regenerated cellulose fiber, characterized in that: The steps include: 1) dispersing the functionalized graphene in an ionic liquid to obtain a functionalized graphene dispersion; 2) mixing the initial cellulose with the functionalized graphene dispersion obtained in step 1) to obtain a cellulose spinning solution; 3) spinning the cellulose spinning solution obtained in step 2) to obtain regenerated cellulose fibers; Wherein, the functionalized graphene is selected from at least one of amino graphene, hydroxylated graphene and fluorinated graphene; Wherein, the initial cellulose is selected from wood pulp cellulose and / or cotton pulp cellulose; Wherein, the mass ratio of the functionalized graphene to the initial cellulose is 0.05 to 5:
100.
2. The preparation method according to claim 1, characterized in that: In step 1), the mass ratio of the functionalized graphene to the ionic liquid is 0.003-0.015:40-60.
3. The preparation method according to claim 1, characterized in that: The ionic liquid is an imidazole ionic liquid.
4. The preparation method according to claim 1, characterized in that: The ionic liquid is selected from one of 1-allyl-3-methylimidazolium chloride, 1-butyl-3-methylimidazolium chloride, 1-ethyl-3-methylimidazolium acetate and 1-ethyl-3-methylimidazolium chloride.
5. The preparation method according to claim 1, characterized in that: The ionic liquid is 1-allyl-3-methylimidazolium chloride.
6. The preparation method according to claim 1, characterized in that: The mass ratio of the functionalized graphene to the initial cellulose is 0.1 to 1:100; in step 2), the mixing temperature is 40 to 85°C.
7. The preparation method according to claim 1, characterized in that: In step 1) and step 2), no dispersant is added.
8. The preparation method according to claim 1, characterized in that: In step 3), the cellulose spinning solution obtained in step 2) is degassed, the degassed cellulose spinning solution is ejected through a spinneret, formed in a coagulation bath, and then washed, dried and oiled to obtain regenerated cellulose fibers.
9. A regenerated cellulose fiber, characterized in that It is prepared according to the preparation method according to any one of claims 1 to 8.
10. Use of the regenerated cellulose fiber according to claim 9 in preparing carbon fiber.
Citation Information
Patent Citations
Graphene blend regenerated cellulose fiber and preparation method thereof
CN103046151A
Functional cellulose fiber containing graphene and preparation method thereof
CN105603554A
Fusion-method-prepared functional graphene cellulose fiber and preparation method thereof
CN106149083A
Graphene modified cellulose membrane and preparation method thereof
CN107417937A
Preparation method of multifunctional regenerated cellulose composite fiber
CN108277545A