High-compactness carbon fiber and preparation method thereof

By using the chemical reaction between the uniform sulfonated graphene and polymer of the sulfonated graphene in the preparation of carbon fiber, the hole problem caused by uneven functional groups is solved, and the preparation of carbon fiber with high density and high performance is achieved .

CN118932553APending Publication Date: 2024-11-12SUZHOU GRAPHENE NEW MATERIAL TECH +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411292750.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In traditional carbon fiber preparation methods, uneven distribution of functional groups on the surface of graphene leads to the formation of holes, limiting the improvement of the strength and performance of carbon fibers.

Method used

Using sulfonated graphene, the polymer polymer forms a uniform chemical bond with graphene through the uniform distribution of sulfonated groups, and is subjected to spinning, pre-carbonization and graphitization to form highly dense carbon fibers.

Benefits of technology

The high density and high graphitization of carbon fibers are achieved, which significantly improves its strength and thermal conductivity and reduces the cross-sectional porosity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932553A_ABST
    Figure CN118932553A_ABST
Patent Text Reader

Abstract

The invention discloses a high-compactness carbon fiber and a preparation method thereof. The preparation method comprises the following steps: providing sulfonated graphene, wherein sulfonated groups of the sulfonated graphene are uniformly distributed on a graphene matrix; the sulfonation group is compounded with a selected high-molecular polymer to form a spinning solution, the selected high-molecular polymer has a selected group, and the selected group can chemically react with the sulfonation group to generate a chemical bond; spinning to obtain precursor fibers; and carrying out pre-carbonization treatment and graphitization treatment on the precursor fiber to obtain the high-compactness carbon fiber. According to the preparation method provided by the invention, based on a special structure of sulfonated graphene, by utilizing the characteristics that sulfonated groups in sulfonated graphene are uniformly distributed in graphene and do not have edge concentrated distribution, a high-molecular polymer can be uniformly connected to a graphene sheet layer, and in the cross-linking and carbonization process, the cross-linking and carbonization effects are greatly improved. The fiber structure can be uniformly shrunk to form the fiber with a complete and compact structure, and the graphitization degree is relatively high in the graphitization process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic carbon materials, and in particular to a high-density carbon fiber and a preparation method thereof. Background Art

[0002] Carbon fiber refers to high-strength and high-modulus fiber with a carbon content of more than 90%. It is the best in high temperature resistance among all chemical fibers. Traditional carbon fiber is made of acrylic and viscose fibers, which are oxidized and carbonized at high temperature after spinning. It is an excellent material for manufacturing high-tech equipment such as aerospace.

[0003] A variety of different methods for preparing carbon fibers have been developed in this field. Some studies start from graphene, using the functional groups connected to the surface of graphene to cause a condensation reaction between it and a polymer, so that the polymer and graphene are connected. The combined material is then spun and carbonized and graphitized to obtain graphene-based carbon fibers.

[0004] This type of carbon fiber usually has certain strength and high thermal conductivity, but because the traditional construction method of functional groups on the surface of graphene is based on graphene oxide, its functional groups are usually mainly distributed near the edges of the graphene sheets, which will lead to uneven reaction problems during condensation and subsequent carbonization and graphitization, thereby causing the formation of holes, which in turn limits the strength of the prepared carbon fiber and the improvement of various other properties. Summary of the invention

[0005] In view of the deficiencies in the prior art, an object of the present invention is to provide a high-density carbon fiber and a preparation method thereof.

[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes: In a first aspect, the present invention provides a method for preparing a high-density carbon fiber, comprising: Providing sulfonated graphene, wherein the sulfonated graphene comprises a graphene matrix and a sulfonated group bonded to the graphene matrix, and the sulfonated group is uniformly distributed on the graphene matrix; Compounding the sulfonated graphene with a selected high molecular polymer to form a spinning solution, wherein the selected high molecular polymer has a selected group, and the selected group can chemically react with the sulfonated group to generate a chemical bond; Spinning with the spinning solution to obtain precursor fibers; The precursor fiber is subjected to pre-carbonization treatment and graphitization treatment to obtain a high-density carbon fiber.

[0007] In a second aspect, the present invention also provides a high-density carbon fiber obtained by the above preparation method, wherein the cross-sectional porosity of the high-density carbon fiber is less than 2%.

[0008] Based on the above technical solution, compared with the prior art, the beneficial effects of the present invention at least include: The preparation method provided by the present invention is based on the special structure of sulfonated graphene, and utilizes the characteristics that the sulfonated groups in the sulfonated graphene are evenly distributed in the graphene and do not have the edge concentrated distribution trend, so that the high molecular polymer can be evenly connected to the graphene sheet layer. During the crosslinking and carbonization process, the fiber structure will produce uniform shrinkage to form a fiber with a complete and dense structure, and the graphitization process also has a high degree of graphitization, which is very helpful for improving the strength and thermal conductivity of carbon fiber and other properties.

[0009] The above description is only an overview of the technical solution of the present invention. In order to enable those skilled in the art to more clearly understand the technical means of the present application and implement them according to the contents of the specification, the following is a description of the preferred embodiments of the present invention in conjunction with detailed drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1a It is a schematic diagram of the functional group distribution state of functionalized graphene used in some prior arts of the present invention; Figure 1b Schematic diagram of functional group distribution state of sulfonated graphene used in some typical implementation cases of the present invention; Figure 2 This is a low-magnification scanning electron microscope photograph of a cross section of a high-density carbon fiber provided in a typical embodiment of the present invention; Figure 3 This is a high-magnification scanning electron microscope photograph of a cross section of a high-density carbon fiber provided in a typical embodiment of the present invention; Figure 4 This is a high-magnification scanning electron microscope photo of a cross section of a carbon fiber provided in a typical comparative example of the present invention; Figure 5 This is a graph showing the degree of graphitization of high-density carbon fiber provided in a typical implementation example of the present invention. DETAILED DESCRIPTION

[0011] In view of the deficiencies in the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution, its implementation process and principle will be further explained as follows.

[0012] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.

[0013] Moreover, relational terms such as “first” and “second” are merely used to distinguish one component or method step from another with the same name, but do not necessarily require or imply any such actual relationship or order between these components or method steps.

[0014] The embodiment of the present invention provides a method for preparing high-density carbon fiber, which comprises the following steps: Providing sulfonated graphene, wherein the sulfonated graphene comprises a graphene matrix and a sulfonated group bonded to the graphene matrix, and the sulfonated group is uniformly distributed on the graphene matrix; Compounding the sulfonated graphene with a selected high molecular polymer to form a spinning solution, wherein the selected high molecular polymer has a selected group, and the selected group can chemically react with the sulfonated group to generate a chemical bond; Spinning with the spinning solution to obtain precursor fibers; The precursor fiber is subjected to pre-carbonization treatment and graphitization treatment to obtain a high-density carbon fiber.

[0015] The sulfonated graphene used in the present invention is a quasi-two-dimensional material, similar to graphene oxide and graphene, and is a carbon material with sulfonic acid or sulfonate functional groups chemically bonded. In the art, the terms "sulfonated graphene", "sulfonated carbon material" or "carbon material containing sulfonate functional groups" have similar meanings and can be used interchangeably. A key feature of the sulfonated graphene used in the present invention is that the sulfonated groups on its surface are evenly distributed and do not tend to be concentrated toward the edge of the graphene sheet.

[0016] Pre-carbonization treatment can also be expressed as pre-oxidation treatment, carbonization treatment or heat treatment in some technical solutions in the field. The process of cross-linking and carbonization of sulfonated graphene and selected polymers is achieved in this process; and graphitization treatment is also a common process in carbon fiber preparation, which uses higher temperatures to prompt carbon elements to form graphite structures.

[0017] In the present invention, the sulfonated graphene used is a graphene functionalized material different from general functionalized graphene. Figure 1a As shown, conventional functionalized graphene, such as amino graphene or carboxyl graphene, etc., are prepared by oxidation, reduction or substitution reaction of graphene oxide, and the distribution state of its functional groups is based on the distribution of oxidized groups in graphene oxide. In conventional graphene oxide preparation methods, oxidized groups are usually concentrated at the edge of graphene sheets, which should be related to the steric hindrance effect and the higher activity of more edge defects. Therefore, the functionalized groups of the prepared functionalized graphene are also concentrated at the edge of graphene, unlike the method used in the present invention. Figure 1bAs shown in the sulfonated graphene, the sulfonated groups are evenly distributed in the central region and the surrounding edge regions of the graphene.

[0018] Based on the above problems, some prior arts propose a carbon fiber preparation scheme in which functionalized graphene is combined with a polymer spinning carbonization and graphitization, such as the Chinese invention patent with publication number CN117364299A, which uses graphene oxide for amino modification, and then combines it with a polymer that can react with amino groups to form chemical bonds, to form original fibers by spinning, and then use traditional carbonization and graphitization methods to form carbon fibers. Since its functional groups are mainly distributed at the edges (i.e., they tend to be concentrated at the edges, for example, more than 80% of the functional groups are concentrated at the edges of the graphene sheets), an uneven reaction occurs during the cross-linking carbonization process, which leads to the generation of holes. The holes have a significant effect on the strength, thermal conductivity, and electrical conductivity of carbon fibers, because these properties are all related to the effective cross-sectional area of ​​the fiber, and the holes occupy the cross-sectional area but cannot provide load or conduction capacity.

[0019] The significant improvement of the present invention is that the functional groups are evenly distributed on the surface of the carbon hexacyclic ring, and the carbon hexacyclic ring of the sulfonated graphene prepared based on previous research has higher integrity and significantly lower edge defects. Therefore, in the process of attempting to prepare carbon fiber, it is found that based on the characteristics of the above functional groups, a uniform and obvious self-shrinkage phenomenon will occur during the crosslinking and carbonization process, the structure will spontaneously become denser, and the later graphitization strength will also be higher, thereby providing a sufficient upper limit for the improvement of various performances, which is currently impossible to achieve with the aforementioned methods, and the mechanism of densification shrinkage brought about by the sulfonated graphene with the above characteristics is also a new discovery.

[0020] As to how to obtain the sulfonated graphene, in some embodiments, the sulfonated graphene is formed by stepwise oxidation and sulfonation of an organic material by an oxidative sulfonating agent.

[0021] More specifically, in some embodiments, the formation process of sulfonated graphene may include the following process flow: A reaction medium containing the oxidative sulfonating agent is contacted with the organic material at a first temperature.

[0022] The reaction temperature is increased to a second temperature to allow the oxidative sulfonating agent to continue reacting with the organic material, thereby obtaining the sulfonated graphene.

[0023] The first temperature is from the melting temperature of the organic material to lower than the boiling point of the reaction medium, and the second temperature is above the boiling point of the reaction medium.

[0024] Regarding the selection of raw materials for the above-mentioned synthesis process, in some embodiments, the organic material includes polyethylene wax, polyacetylene, polyalkynes containing halogen elements, polyethylene, polyolefins containing halogen elements, C4-C 50 Any one of straight-chain hydrocarbons and aromatic hydrocarbons with a benzene ring structure, or a combination of two or more thereof.

[0025] In some embodiments, the oxidative sulfonating agent includes a compound of the general formula R-SO3H, wherein R is selected from F, Cl, Br; a combination of H2SO4 and HCl; a combination of H2SO4 and HF; concentrated sulfuric acid; fuming sulfuric acid; and combinations thereof.

[0026] Regarding the source of sulfonated graphene, reference may be made to some disclosed prior arts, such as the Chinese invention patent with publication number CN105764839A, but it is not limited thereto. The key technical feature utilized in the present invention lies in the structural characteristics of the sulfonated graphene, and is not limited to how to prepare the sulfonated graphene. This means that even if the desired sulfonated graphene is obtained by adopting a preparation idea different from the above examples and the prior art, as long as the sulfonated graphene used has the key structural features indicated in the present invention and produces corresponding effects, the basic technical concept of the present invention has been utilized and is also within the feasible implementation scope of the present invention.

[0027] In addition to sulfonated graphene, in some embodiments of the selected high molecular polymer, the selected group includes any one of amino, hydroxyl, carboxyl, and ester groups, or a combination of two or more thereof.

[0028] Specifically, in some embodiments, the selected high molecular polymer includes any one or a combination of two or more of polyaniline, poly(allylamine), polyvinyl alcohol, hydroxyl polyurethane polymer, polylactic acid-glycolic acid copolymer, polyacrylic acid, and polyacrylate.

[0029] As for specific preparation condition parameters, in some embodiments, the concentration of sulfonated graphene in the spinning solution is 1-150 g / L, and the concentration of the selected high molecular polymer is 1-150 g / L.

[0030] In some embodiments, the spinning material is formed into the precursor fiber by solution spinning or electrospinning; the spinning solution temperature of the solution spinning or electrospinning is -20-50°C.

[0031] In some embodiments, the pre-carbonization treatment is performed at a temperature of 300-1500° C. for 3-24 hours; and the graphitization treatment is performed at a temperature of 2000-3200° C. for 12-48 hours.

[0032] The above condition parameters are the parameter ranges of the preferred examples of the present invention, and do not mean that similar technical effects of improving density cannot be achieved beyond the above exemplary ranges. It should also be noted that the solution (or dispersion) in the spinning solution is not required, and any solvent that can disperse and dissolve the sulfonated carbon fiber and the selected polymer, and can be volatilized and removed during the spinning process to form the silk thread can be used in the spinning process.

[0033] Another aspect of the embodiment of the present invention further provides a high-density carbon fiber prepared by the above-mentioned preparation method, wherein the cross-sectional porosity of the high-density carbon fiber is less than 2%. The high-density carbon fiber prepared by the preparation method provided by the present invention has the characteristic of being almost free of pores, while the carbon fiber prepared by the existing traditional technical solution is usually very difficult to achieve a cross-sectional porosity of less than 2%.

[0034] As shown above, a notable feature of the carbon fiber prepared by the present invention is its extremely high density, which is an outstanding structural feature brought about by the selected sulfonated graphene with certain structural characteristics combined with polymer spinning, carbonization and graphitization, and is a feature that is difficult to obtain by existing carbon fiber preparation methods.

[0035] The technical solution of the present invention is further described in detail below through several embodiments and in conjunction with the accompanying drawings. However, the selected embodiments are only used to illustrate the present invention, and do not limit the scope of the present invention.

[0036] Example 1 This embodiment illustrates a preparation process of a high-density carbon fiber, which is specifically as follows: 1. Preparation of sulfonated graphene: In a fume hood, add 600 g of 99% pure chlorosulfonic acid as a reaction medium to an open 2-liter three-necked glass reactor, heat the reactor to 50°C using an oil bath, and maintain the temperature, add 10 g of hexadecane, react for 3 hours, then slowly raise the temperature to 160°C, and react at a constant temperature for 12 hours, cool the reaction, filter the contents of the reactor, and wash with deionized water to obtain 9 g of sulfonated graphene product, which is a yellow-brown powder.

[0037] 2. Prepare spinning solution: disperse or dissolve the sulfonated graphene and polyaniline (molecular weight of 10,000-15,000) in step 1 in ethanol solvent to form a spinning solution, wherein the concentration of the sulfonated graphene is 50 g / L and the concentration of the polyaniline is 30 g / L.

[0038] 3. Electrospinning: Using an electrospinning machine, set appropriate parameters for spinning to obtain precursor fibers, the diameter of which is 15 μm.

[0039] 4. Pre-carbonization treatment: The precursor fiber is sent into a heating furnace, first raised to 500°C at 5°C / min, kept warm for 1 hour, then raised to 1200°C at 3°C / min, kept warm for 2 hours.

[0040] 5. Graphitization treatment: The pre-carbonized fiber is sent into a graphitization furnace at a temperature of 2500°C for 36 hours to finally obtain a high-density carbon fiber.

[0041] Figure 2 and Figure 3 The cross-sectional scanning electron microscope photos of the high-density carbon fiber obtained in this embodiment at different magnifications are shown. It can be seen that the carbon fiber obtained in this embodiment has an extremely dense internal structure. No holes or gaps are observed in either a large field of view (low magnification) or a local field of view (high magnification). Figure 5 The graphitization degree of the carbon fiber prepared in this embodiment is shown, and it can be seen that it also has a significant advantage in terms of graphitization degree.

[0042] Comparative Example 1 This comparative example illustrates a process for preparing carbon fiber based on graphene oxide, which is specifically as follows: 1. Commercially purchased graphene oxide is then used to aminate the oxidized groups in the graphene oxide using ethylenediamine in a hydrothermal reaction to form aminated graphene.

[0043] 2. Prepare spinning solution: disperse or dissolve the amino graphene and polyacrylonitrile in step 1 in DMSO solvent to form a spinning solution, wherein the concentration of the amino graphene is 30 g / L, and the concentration of the polyacrylonitrile is 30 g / L.

[0044] The subsequent steps are exactly the same as steps 3-5 in Example 1.

[0045] The cross-sectional scanning electron microscope photograph of the carbon fiber prepared in this comparative example is as follows: Figure 4 As shown, obvious holes and gaps can be seen.

[0046] Comparative Example 2 This comparative example is substantially the same as the above-mentioned Example 1, except that: Commercially available graphene oxide was sulfonated using aminosulfonic acid. The specific process was as follows: graphene oxide and aminosulfonic acid were compounded in a ratio of 1:2, heated to 250°C under nitrogen protection, reacted for 8 hours, and sulfonated graphene oxide was obtained after washing and drying.

[0047] The obtained sulfonated graphene was used to prepare carbon fibers by adopting steps 2-5 which are completely the same as those in Example 1.

[0048] The morphology of the carbon fiber obtained in this comparative example is similar to that of comparative example 1, with obvious holes and gaps.

[0049] Example 2 This embodiment is substantially the same as Embodiment 1, and the main difference is that: In step 2, polyaniline is replaced with polyvinyl alcohol (polymer grade is 1788) and dispersed or dissolved in water to form a spinning solution, wherein the concentration of sulfonated graphene is 50 g / L and the concentration of polyvinyl alcohol is 50 g / L.

[0050] In step 4, pre-carbonization treatment: the precursor fiber is placed in a heating furnace, first heated to 500°C at 5°C / min, kept warm for 1 hour, then heated to 1000°C at 3°C / min, kept warm for 2 hours.

[0051] In step 5, the graphitization temperature is 2800° C. and the time is 48 hours, and finally high-density carbon fiber is obtained.

[0052] The cross-sectional morphology of the high-density carbon fiber obtained in this embodiment is the same as that in embodiment 1, and it still has the characteristic of being extremely dense, and the degree of graphitization is also at the same level as that in embodiment 1.

[0053] Example 3 This embodiment is substantially the same as Embodiment 1, and the main difference is that: In step 2, polyaniline is replaced with polyacrylic acid (molecular weight 8000-15000) and dispersed or dissolved in water to form a spinning solution, wherein the concentration of sulfonated graphene is 75 g / L and the concentration of polyacrylic acid is 30 g / L (different concentrations are adjusted).

[0054] In step 4, pre-carbonization treatment: the precursor fiber is placed in a heating furnace, first heated to 500°C at 5°C / min, kept warm for 1 hour, then heated to 900°C at 3°C / min, kept warm for 1 hour.

[0055] In step 5, the graphitization temperature is 3000° C. and the time is 40 h, and finally high-density carbon fiber is obtained.

[0056] The cross-sectional morphology of the high-density carbon fiber obtained in this embodiment is the same as that in embodiment 1, and it still has the characteristic of being extremely dense, and the degree of graphitization is also at the same level as that in embodiment 1.

[0057] Example 4 This embodiment is substantially the same as Embodiment 1, and the main difference is that: In step 3, the spinning method is replaced with solution spinning, the spinning temperature is 80 degrees Celsius, the solution concentration is 8%, and the obtained fiber diameter is 10 microns.

[0058] The cross-sectional morphology of the high-density carbon fiber obtained in this embodiment is the same as that in embodiment 1, and it still has the characteristic of being extremely dense, and the degree of graphitization is also at the same level as that in embodiment 1.

[0059] Based on the above embodiments and comparative examples, it can be clearly seen that the preparation method provided by the present invention is based on the special structure of sulfonated graphene, and utilizes the characteristics of the sulfonated groups in the sulfonated graphene being evenly distributed in the graphene without the trend of edge concentrated distribution, so that the high molecular polymer can be uniformly connected to the graphene sheet. During the crosslinking and carbonization process, the fiber structure will produce uniform shrinkage to form a complete and dense fiber, and it also has a high degree of graphitization during the graphitization process.

[0060] It should be understood that the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing high-density carbon fiber, characterized in that: include: Providing sulfonated graphene, wherein the sulfonated graphene comprises a graphene matrix and a sulfonated group bonded to the graphene matrix, and the sulfonated group is uniformly distributed on the graphene matrix; Compounding the sulfonated graphene with a selected high molecular polymer to form a spinning solution, wherein the selected high molecular polymer has a selected group, and the selected group can chemically react with the sulfonated group to generate a chemical bond; Spinning with the spinning solution to obtain precursor fibers; The precursor fiber is subjected to pre-carbonization treatment and graphitization treatment to obtain a high-density carbon fiber.

2. The preparation method according to claim 1, characterized in that: The sulfonated graphene is formed by stepwise oxidation and sulfonation of an organic material by an oxidative sulfonating agent.

3. The preparation method according to claim 2, characterized in that: The formation process of the sulfonated graphene specifically includes: contacting a reaction medium containing the oxidative sulfonating agent with the organic material at a first temperature; Raising the reaction temperature to a second temperature to allow the oxidative sulfonating agent to continue reacting with the organic material, thereby obtaining the sulfonated graphene; The first temperature is from the melting temperature of the organic material to lower than the boiling point of the reaction medium, and the second temperature is above the boiling point of the reaction medium.

4. The preparation method according to claim 3, characterized in that: The organic material includes polyethylene wax, polyacetylene, polyalkyne containing halogen elements, polyethylene, polyolefin containing halogen elements, C4-C 50 Any one or a combination of two or more of straight-chain hydrocarbons and aromatic hydrocarbons with a benzene ring structure; And / or, the oxidizing sulfonating agent includes a compound of the general formula R-SO3H, wherein R is selected from F, Cl, Br; a combination of H2SO4 and HCl; a combination of H2SO4 and HF; concentrated sulfuric acid; fuming sulfuric acid; and combinations thereof.

5. The preparation method according to claim 1, characterized in that: The selected group includes any one of amino, hydroxyl, carboxyl and ester groups or a combination of two or more thereof.

6. The preparation method according to claim 5, characterized in that: The selected high molecular polymer includes any one or a combination of two or more of polyaniline, poly(allylamine), polyvinyl alcohol, hydroxy polyurethane polymer, polylactic acid-glycolic acid copolymer, polyacrylic acid, and polyacrylate.

7. The preparation method according to claim 1, characterized in that: The concentration of sulfonated graphene in the spinning solution is 1-150 g / L, and the concentration of the selected high molecular polymer is 1-150 g / L.

8. The preparation method according to claim 1 or 7, characterized in that: The spinning material is formed into the precursor fiber by solution spinning or electrostatic spinning; The spinning solution temperature of the solution spinning or electrostatic spinning is -20-50°C.

9. The preparation method according to claim 1, characterized in that: The temperature of the pre-carbonization treatment is 300-1500° C., and the time is 3-24 hours; the temperature of the graphitization treatment is 2000-3200° C., and the time is 12-48 hours.

10. The high-density carbon fiber obtained by the preparation method according to any one of claims 1 to 9, characterized in that: The cross-sectional porosity of the high-density carbon fiber is less than 2%.

Citation Information

Patent Citations

  • Method for preparing sulfonated graphene from organic material and the sulfonated graphene

    CN105764839A

  • Graphene modified composite carbon fibers as well as preparation method and application thereof

    CN106676678A

  • Sulfonated graphene reinforced carbon-based composite material as well as preparation method and application thereof

    CN116283333A

  • Continuous graphene fibers from functionalized graphene sheets

    WO2019222175A1