Production method of regenerated anti-perspective and anti-ultraviolet DTY (Draw Textured Yarn)

By optimizing the process of anti-perspective regeneration semi-optical POY and modifying TiO2, combined with the improved oiling device, the existing fibers have been solved in the problem of insufficient shielding effect and ultraviolet resistance, and a combination of anti-perspective and ultraviolet resistance functions have been prepared. Fiber fills the market gap and improves mechanical properties.

CN118932566APending Publication Date: 2024-11-12浙江佳人新材料有限公司
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410797082.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing anti-perspective DTY fibers and anti-ultraviolet DTY fibers each lack good comprehensive performance, especially the shielding effect and anti-perspective properties of light and thin white fabrics, which is difficult to meet market demand.

Method used

Using a production method of regeneration, anti-perspective and anti-ultraviolet DTY, the anti-perspective regeneration semi-optical POY is stretched, heated and deformed, cooling, false twisting, network and shaped, and TiO2 is added to the fiber to form a W-shaped cross-section. , combined with an improved oiling device, the oil agent filtering and impurity removal ensures that the fiber has both anti-sight and anti-UV functions, and improves mechanical properties.

Benefits of technology

The prepared fibers have good light shading, opacity and UV resistance. The process is simple and easy to operate, filling the market gap, and are suitable for a wide range of application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932566A_ABST
    Figure CN118932566A_ABST
Patent Text Reader

Abstract

The invention discloses a production method of regenerated anti-perspective and anti-ultraviolet DTY (Draw Textured Yarn), which comprises the following steps of: introducing anti-perspective regenerated semi-gloss POY (Polyester Pre-Oriented Yarn) through a raw yarn frame, feeding into a roller I for stretching, inputting into a deformation hot box for heating deformation, cooling through a cooling plate, false twisting through a false twister, stretching through a roller II, networking, heating and shaping through a shaping hot box, oiling through an oiling device, and finally winding and forming. The regenerated anti-perspective and anti-ultraviolet DTY is prepared. The fiber has anti-perspective and anti-ultraviolet functions and has good mechanical properties, the technological method is simple and easy to operate, and the market blank is filled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of fiber technology, and more specifically to a production method of regenerated anti-see-through and anti-ultraviolet DTY. Background Art

[0002] In the prior art, anti-see-through DTY fiber and anti-ultraviolet DTY fiber are two different functional yarns, which are realized by adding anti-see-through masterbatch and anti-ultraviolet masterbatch respectively. Anti-see-through DTY fiber does not have good anti-ultraviolet property, and the shielding effect of anti-see-through DTY fiber is sometimes difficult to meet the requirements, especially for thin white fabrics, the shielding effect is usually poor, and anti-ultraviolet DTY fiber usually does not have good anti-see-through property; anti-see-through DTY fiber and anti-ultraviolet DTY fiber each have their own shortcomings. If the fiber with both anti-see-through and anti-ultraviolet properties can be prepared through innovative process methods, it will have a broader application scenario and market demand. Summary of the invention

[0003] The purpose of the present invention is to overcome the deficiencies of the above-mentioned prior art and provide a production method of regenerated anti-perspective and anti-ultraviolet DTY. The fiber has both anti-perspective and anti-ultraviolet functions and good mechanical properties. The process method is simple and easy to operate, filling the market gap.

[0004] In order to achieve the above object, the present invention adopts the following technical solution:

[0005] A production method for regenerated anti-see-through and anti-ultraviolet DTY, wherein the anti-see-through regenerated semi-gloss POY is introduced through a raw yarn rack, fed into a first roller for stretching, and then input into a deformation hot box for heating and deformation, and then cooled by a cooling plate, false twisted by a false twister, stretched by a second roller, networked, heated and shaped in a shaping hot box, and then oiled by an oiling device, and finally wound and formed, so as to obtain the regenerated anti-see-through and anti-ultraviolet DTY.

[0006] Furthermore, the cross section of the anti-see-through regenerated semi-bright POY is W-shaped.

[0007] Furthermore, the TiO2 content in the anti-see-through regenerated semi-gloss POY is 1-2%.

[0008] Furthermore, the temperature of the deformation hot box is 160°C to 180°C.

[0009] Furthermore, the stretching ratio is 1.7 to 1.76.

[0010] Furthermore, the processing speed is 550-650 m / min.

[0011] Furthermore, the D / Y ratio is 1.65 to 1.68.

[0012] Furthermore, the temperature of the shaping hot box is 160-170°C.

[0013] The beneficial effects of the present invention are:

[0014] Using W-shaped cross-section anti-see-through recycled semi-gloss POY as raw material, the recycled anti-see-through and anti-UV DTY is prepared through the optimization and improvement of the texturizing process. Through titanium dioxide modification, the fiber can have both anti-see-through and anti-UV functions, and has good mechanical properties. The process is simple and easy to operate, filling the market gap. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 A schematic diagram of the structure of the improved oiling device in Example 2;

[0016] Figure 2 for Figure 1 The enlarged view of point A in the middle;

[0017] Figure 3 This is a schematic diagram of the process of the improved oiling device in Example 2 driving the filter element to remove impurities from the oil.

[0018] Figure numerals: box body 1, partition plate 11, through hole 111, upper chamber 12, lower chamber 13, baffle 14, oil roller 2, filter element 3, sealing plate 31, filter screen 32, sealing block 4, dust collector head 5, first cylinder 6, connecting rod 61, second cylinder 7. DETAILED DESCRIPTION

[0019] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] The production method of the regenerated anti-perspective and anti-ultraviolet DTY of the present invention is as follows: the anti-perspective regenerated semi-gloss POY is introduced through a raw yarn frame, fed into a roller for stretching, and then input into a deformation hot box for heating and deformation, and then cooled by a cooling plate, false twisted by a false twister, stretched by two rollers, networked, heated and shaped in a shaping hot box, and then oiled by an oiling device, and finally wound and formed to obtain the regenerated anti-perspective and anti-ultraviolet DTY. The cross section of the anti-perspective regenerated semi-gloss POY is W-shaped. The anti-perspective regenerated semi-gloss POY is self-made by Zhejiang Jiaren New Materials Co., Ltd., and the TiO2 content in the anti-perspective regenerated semi-gloss POY is 1-2%. The temperature of the deformation hot box is 160°C to 180°C; the stretching multiple is 1.7 to 1.76; the processing speed is 550 to 650 m / min; and the D / Y ratio is 1.65 to 1.68.

[0021] Example 1

[0022] Production of recycled anti-see-through and anti-ultraviolet DTY

[0023] The anti-perspective regenerated semi-gloss POY (linear density: 35.99 dtex; linear density CV: -1.33%; breaking strength: 2.10 cN / dtex; strip CV: 0.90%) is introduced through the raw yarn rack, fed into a roller for stretching, and then input into the deformation hot box for heating and deformation, and then cooled by a cooling plate, false twisted by a false twister, stretched by two rollers, networked, heated and shaped in a shaping hot box, and then oiled by an oiling device, and finally wound and formed to obtain a regenerated anti-perspective and anti-ultraviolet DTY. The cross section of the anti-perspective regenerated semi-gloss POY is W-shaped. The anti-perspective regenerated semi-gloss POY is made by Zhejiang Jiaren New Materials Co., Ltd., and the TiO2 content in the anti-perspective regenerated semi-gloss POY is 1-2%. The temperature of the deformation hot box is 170°C; the stretching multiple is 1.735; the processing speed is 600m / min; and the D / Y ratio is 1.65.

[0024] The anti-see-through regenerated semi-gloss POY is specifically prepared by the following method:

[0025] (a) The regenerated semi-matt polyester chips are crystallized and dried (crystallization temperature is 158°C, drying temperature is 165°C, and drying air pressure is 0.1 MPa), and then blended with matt masterbatch through a two-component automatic batching machine (the matt masterbatch is a polyester masterbatch with a titanium dioxide content of 2.5%, and the TiO2 content in the final anti-transmission regenerated semi-matt POY is controlled to be 1.1%), and the mixture is transported to a screw extruder for melt extrusion (the diameter of the screw extruder is 6 5mm, aspect ratio is 25, heating temperature of zones 1 to 5 is 277℃ for zone 1, 283℃ for zone 2, 285℃ for zone 3, 288℃ for zone 4 and 288℃ for zone 5 respectively, extrusion pressure of screw extruder is 11.1Mpa, pressure after filtration is 9.4Mpa), and then the melt is transported to spinning box, and after metering by metering pump, it is pressed into spinning assembly for spinning to form primary filament bundle, pump supply of metering pump is 21.5g / min, and spinning temperature is 290℃. The spinning assembly includes spinneret, the material outlet cross section of spinneret is W-shaped, the material outlet cross section is formed by four leaves connected into W shape, the angle between two connected leaves is 60°, each leaf is 0.28mm long and 0.07mm wide.

[0026] (b) The spun filament bundle is subjected to post-heating, windless zone cooling, annular air cooling, and bundle oiling treatment, and then pre-networking, drawing and shaping, and winding to obtain a special-shaped cross-section anti-transmission regenerated semi-optical fiber. The post-heating temperature is 300°C, the windless zone height is 46mm, the wind pressure of the annular air cooling is 40Pa; the oil concentration ratio is 11.1%; the pre-network pressure is 0.07Mpa; the speed of the first drafting roller during drawing and shaping is 2650m / min, and the speed of the second drafting roller is 2730m / min; the winding speed during winding is 2870m / min, and the winding tension is 8.1cN.

[0027]

[0028] Example 2

[0029] Regenerated anti-perspective and anti-ultraviolet DTY was prepared according to the method of Example 1, but an improved oiling device was used (the oiling device of Example 1 is a traditional oil roller oiling device, the oil roller is immersed in the oil agent, and the fiber passes through the lower end of the oil roller for oiling). However, in this traditional oiling process, the oil agent is stored statically in the oil storage tank, the oil agent will precipitate or the oil agent will partially solidify, and the fiber will bring dust, lint and other impurities into the oil agent during the oiling process, resulting in impurities in the oil agent, affecting the oiling quality. Although the oil agent can be circulated and transported to the filter screen for filtration, as the impurities adsorbed on the filter screen gradually increase, it will gradually have an adverse effect on the oiling quality, and the filter screen must be stopped for cleaning after a period of production, which is not conducive to continuous production and ensuring production efficiency.

[0030] like Figure 1-3 As shown, the improved oiling device comprises a box body 1, an oil roller 2 rotatably mounted in the box body 1, and a filter element 3 embedded in the inner cavity of the box body 1 and sealingly and slidably connected to the inner wall of the box body 1. The box body 1 is divided into an upper chamber 12 and a lower chamber 13 distributed up and down by a fixed partition plate 11. The oil roller 2 and the filter element 3 are both installed in the upper chamber 12. The filter element 3 is located below the oil roller 2. The back-and-forth movement direction of the filter element 3 is perpendicular to the axial direction of the oil roller 2. The filter element 3 comprises an inverted T-shaped sealing plate 31 and filter screens 32 respectively fixedly mounted on the two side walls of the vertical part of the sealing plate 31. The upper inner walls of both sides of the box body 1 are fixedly mounted. There is a baffle 14, and the filter element 3 moves to the lower part of the sealing plate 31 to abut against the inner wall of the box body 1, so that the sealing plate 31 is sealed and connected with the lower end surface of the baffle 14 and the inner wall of the box body 1; the lower chamber 13 is respectively embedded with two sealing blocks 4 that are slidably connected to the inner wall of the lower chamber 13, and the two ends of the partition plate 11 are respectively provided with through holes 111; initially, the filter element 3 is located at one side of the box body 1 and is sealed with the baffle 14 on one side, and the bottom of the sealing plate 31 covers the through hole 111 on one side, and the two sealing blocks 4 are respectively located at the two ends of the lower chamber 13 and block the through hole 111, that is, the two sealing blocks 4 are in an extended state, such as Figure 1 , Figure 2 As shown, a plurality of dust collecting heads 5 are respectively installed on the box walls on both sides of the box body 1, and each dust collecting head 5 is connected to a dust collector (not shown in the figure). The sealing plate 31 and the sealing block 4 can maintain a seal with the contacting wall in the moving or stationary state.

[0031] The top height of the sealing plate 31 is lower than the bottom height of the oil roller 2. The sealing plate 31 is preferably completely covered with a layer of sealing material (such as rubber) on the surface of the inverted T-shaped hard plate; the top height of the vertical part of the sealing plate 31 is higher than the top height of the filter screen 32. The filter screens 32 on both sides of the sealing plate 31 and the horizontal part of the sealing plate 31 form a step-like structure, that is, the filter screen 32 does not exceed the outer end of the horizontal part of the sealing plate 31, so that when the horizontal part of the sealing plate 31 moves to abut the inner wall of the box body 1, there is a certain gap between the filter screen 32 and the inner wall of the box body 1, such as Figure 1 , Figure 2 As shown, the dust collector head 5 is helpful to absorb impurities on the filter screen 32.

[0032] The filter element 3 is driven to move back and forth by the first cylinder 6 , the axial end of the first cylinder 6 is connected to the filter element 3 through a connecting rod 61 , and the two sealing blocks 4 are driven to move back and forth by the second cylinder 7 respectively.

[0033] When the oiling device is in the above initial state (such as Figure 1 As shown in the figure, oil is injected into the upper chamber 12 and partially submerged in the oil roller 2. The fiber passes through the lower end of the oil roller 2 and begins to be oiled. After a period of oiling, the oil contains certain impurities, which drives the filter element 3 to move to the other side (as shown in the figure). Figure 3 (a) is for reference, that is, moving to the right side). During the movement of the filter element 3, impurities in the oil agent will adhere to the filter screen 32, especially the filter screen 32 on the right side. When the filter element 3 moves to the point where the sealing plate 31 is in sealing contact with the baffle plate 14 on the other side but the sealing plate 31 does not completely cover the through hole 111 on the other side (a plurality of through holes 111 can be provided along the axial direction of the oil roller 2), the filter element 3 is stopped from moving. Figure 3 As shown in (b), the sealing block 4 on the other side is driven to move backward (i.e., move to the left) to form a receiving chamber between the sealing block 4 and the inner wall of the box body 1, so that the upper chamber 12 and the lower chamber 13 at the front end of the sealing block 4 are connected through the through hole 111 on the other side, and the oil in the outer chamber of the filter element 3 flows into the receiving chamber through the through hole 111. After the oil in the outer chamber of the filter element 3 has completely flowed out, the filter element 3 is driven to continue to move to the other side until the filter element 3 abuts against the inner wall of the box body 1 and covers the through hole 111 on this side. Figure 3As shown in (c), the side dust collector 5 is then driven to remove the impurities on the outer filter 32. After the filter 32 is cleaned, the filter element 3 is started to move back (i.e., move to the left), and at the same time, the side sealing block 4 is driven forward to push the oil in the accommodating chamber back into the upper chamber 12, and the sealing block 4 blocks the through hole 111 on the other side again. When the filter element 3 moves back to the baffle 14 abutting one side, the impurities in the oil will adhere to the filter 32, especially the filter 32 on the left side, and then the filter 32 is cleaned according to the above operation. By moving the filter 32 back and forth, the impurities in the oil are timely adsorbed and the impurities on the filter 32 are removed, achieving oiling and cleaning at the same time, and at the same time, it can play a certain stirring role on the oil to prevent partial solidification, and there is no need to stop work to remove impurities on the filter, thereby improving the oiling quality and production efficiency.

[0034] The white fabric of the fiber prepared by the method of Example 2 has a light shielding rate of 97.02%, an opacity of 99.92%, an ultraviolet transmittance of 4.05%, a breaking strength of 4.1 cN / dtex, a breaking elongation of 30.33%, and a curl stability of 83.2%.

[0035] Comparative Example 1

[0036] The anti-see-through regenerated semi-bright POY was prepared according to the method of the anti-see-through regenerated semi-bright POY in Example 1, but the fiber cross section was cross-shaped, and then the regenerated anti-see-through and anti-ultraviolet DTY was prepared according to the method of Example 1.

[0037] Comparative Example 2

[0038] The anti-see-through regenerated semi-bright POY was prepared according to the method of the anti-see-through regenerated semi-bright POY in Example 1, but the fiber cross section was cross-shaped, and then the regenerated anti-see-through and anti-ultraviolet DTY was prepared according to the method of Example 2.

[0039] The test found that the white fabric of the fiber prepared in Comparative Example 1 had a shading rate of 85.04%, an opacity of 87.91%, an ultraviolet transmittance of 5.26%, a breaking strength of 3.46 cN / dtex, an elongation at break of 24.18%, and a curl stability of 70.38. Compared with Comparative Example 1, the white fabric of the fiber prepared in Comparative Example 2 had a shading rate of 84.13%, an opacity of 88.26%, an ultraviolet transmittance of 5.21%, a breaking strength of 3.92 cN / dtex, and the curl stability was not improved.

[0040] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A method for producing regenerated anti-see-through and anti-ultraviolet DTY, characterized in that: The anti-see-through regenerated semi-gloss POY is introduced through the raw yarn rack, fed into a roller for stretching, and then input into a deformation hot box for heating and deformation. It is then cooled by a cooling plate, false-twisted by a false twister, stretched by two rollers, networked, heated and formed in a shaping hot box, and then oiled by an oiling device. Finally, it is wound and formed to obtain the regenerated anti-see-through and anti-ultraviolet DTY.

2. A method for producing regenerated anti-see-through and anti-ultraviolet DTY according to claim 1, characterized in that: The cross section of the anti-see-through regenerated semi-gloss POY is W-shaped.

3. The method for producing regenerated anti-see-through and anti-ultraviolet DTY according to claim 1, characterized in that: The TiO2 content in the anti-see-through regenerated semi-gloss POY is 1-2%.

4. The method for producing regenerated anti-see-through and anti-ultraviolet DTY according to claim 1, characterized in that: The temperature of the deformation hot box is 160℃~180℃.

5. The method for producing regenerated anti-see-through and anti-ultraviolet DTY according to claim 1, characterized in that: The stretching ratio is 1.7 to 1.

76.

6. The method for producing regenerated anti-see-through and anti-ultraviolet DTY according to claim 1, characterized in that: The processing speed is 550~650m / min.

7. The method for producing regenerated anti-see-through and anti-ultraviolet DTY according to claim 1, characterized in that: The D / Y ratio is 1.65~1.

68.

8. The method for producing regenerated anti-see-through and anti-ultraviolet DTY according to claim 1, characterized in that: The temperature of the hot box is 160-170℃.

Citation Information

Patent Citations

  • Novel chinlon spandex air-coated yarn and production process thereof

    CN104195699A

  • Elasticizer-based production technology processing POY filament into DTY filament

    CN105133107A

  • Anti-transparent and ultraviolet-resistant warp-knitting fabric and purpose of same

    CN105463686A

  • DTY silk containing anti-ultraviolet agents and production process thereof

    CN111850738A

  • Intelligent self-cleaning transformer oil conservator

    CN112614663A