Carbon nanotube yarn braided fabric with electromagnetic shielding function and preparation method thereof

Carbon nanotube yarn braided fabrics were prepared by floating catalytic chemical vapor deposition and automated knitting technology, solving the processing problem of carbon nanotube fibers and realizing carbon nanotube yarn braided fabrics with high flexibility and excellent electromagnetic shielding performance, which are suitable for flexible electronic materials and aerospace.

CN118932591APending Publication Date: 2024-11-12FUDAN UNIVERSITY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410932427.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing carbon nanotube fibers are difficult to process directly into yarns and fabrics, resulting in poor flexibility, low electrical conductivity, and poor dispersion of carbon nanotube powder, which limits their application in fields such as flexible electronic devices and aerospace.

Method used

Carbon nanotube fibers were prepared by floating catalytic chemical vapor deposition and continuously fused and twisted into carbon nanotube yarns. Then, they were woven into fabrics with various structures using automated knitting technology.

Benefits of technology

Continuous fabrication and weaving of various structures of carbon nanotube yarns have been achieved, resulting in carbon nanotube yarn woven fabrics with high flexibility and excellent electromagnetic shielding performance, suitable for flexible electronic materials and aerospace fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932591A_ABST
    Figure CN118932591A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of functional materials, and particularly relates to a carbon nanotube yarn braided fabric with an electromagnetic shielding function and a preparation method of the carbon nanotube yarn braided fabric. The preparation method of the carbon nanotube yarn woven fabric comprises the following steps: preparing carbon nanotube fibers by using a floating catalytic chemical vapor deposition method; continuously combining and twisting the plurality of carbon nanotube fibers into carbon nanotube yarns with a certain twist degree; and weaving the carbon nano tube yarns or the carbon nano tube yarns and common yarns into the carbon nano tube yarn woven fabric through an automatic knitting technology. The fabric has good electromagnetic shielding effectiveness, the average electromagnetic shielding effectiveness can reach 30 dB or above within the X wave band (8.2-12.4 GHz), and the fabric can be used in the fields of national defense equipment, aerospace, high-frequency communication, wearable electronic equipment and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional materials, and in particular relates to a carbon nanotube yarn woven fabric with electromagnetic shielding function and a preparation method thereof. Background Art

[0002] With the vigorous development of electronic equipment and the communications industry, serious electromagnetic interference problems will occur inside and outside electronic equipment and in the surrounding environment. Electromagnetic shielding technology can prevent the failure and performance degradation of electronic equipment, protect human health and the surrounding environment, and is crucial for applications in the fields of electronic information, aerospace, etc. At present, the mainstream electromagnetic shielding materials are mainly metals or metal oxides. For example, in patent CN202410441611.3, researchers mixed Fe3O4, graphite and other materials to prepare electromagnetic shielding materials, which are used to solve the electromagnetic interference, short circuit and breakdown problems between electronic components inside optical communication modules. However, metal materials have problems such as heavy weight, poor flexibility and easy corrosion. Carbon nanomaterials are light in weight and have excellent conductivity, and have great advantages in electromagnetic shielding. Researchers used modified graphene / modified multi-walled carbon nanotubes as conductive composite fillers (CN202410432641.8) to prepare cable materials with electromagnetic shielding functions. Patent CN202110300518.7 prepared carbon nanotube-reinforced aluminum-based composite foam materials for electromagnetic shielding. However, the above methods all disperse carbon nanotubes as fillers in other phases, such as rubber and metal, which will cause the problem of poor dispersion of carbon nanotube powder. In addition, both rubber and metal have the problem of poor corrosion resistance, and the final products are all blocks, which have poor flexibility, portability, and comfort, and low electrical conductivity. Their application is limited in many occasions such as wearable electronic devices. Therefore, a new electromagnetic shielding material with flexibility, light weight and excellent electrical conductivity is needed.

[0003] Carbon nanotube fiber is a macroscopic continuous fiber material with a micrometer diameter constructed by assembling nanoscale carbon nanotubes as units. It has unique properties such as high conductivity, corrosion resistance, high flexibility and light weight, and is expected to become one of the potential substitutes for metal electromagnetic shielding materials. However, due to the scale problem, a single carbon nanotube fiber is difficult to use directly. It needs to be processed into carbon nanotube yarn and fabric before it can be used. However, most of the carbon nanotube yarn woven fabrics reported so far are to coat the carbon nanotube powder dispersion on the polymer yarn and the polymer fabric substrate (J. Mater. Chem. C 2017, 5, 2432-2441.), or to coat the carbon nanotube film on the surface of the polymer yarn and then weave it into a fabric (ACS Nano 2016, 10, 9129–9135.), instead of directly processing and weaving the carbon nanotube fiber. Therefore, the prepared carbon nanotube yarn and fabric have problems such as poor uniformity of carbon nanotubes, which are not suitable for large-scale preparation and application. Therefore, achieving simultaneous twisting of carbon nanotube fibers into yarns and continuous weaving is a challenge in the preparation of carbon nanotube yarn woven fabrics and their subsequent applications. Summary of the invention

[0004] The purpose of the present invention is to provide a carbon nanotube yarn woven fabric with electromagnetic shielding function and a preparation method thereof, in order to realize the large-scale application of carbon nanotube yarn woven fabric in the field of electromagnetic shielding, in order to address the problems of poor flexibility of metal electromagnetic shielding bodies and limited processing and weaving of carbon nanotube fibers into electromagnetic shielding fabrics.

[0005] The method for preparing the carbon nanotube yarn braid with electromagnetic shielding function provided by the present invention comprises the following specific steps:

[0006] First, carbon nanotube fibers were prepared using floating catalytic chemical vapor deposition;

[0007] Then, a plurality of carbon nanotube fibers are continuously combined and twisted into a carbon nanotube yarn with a certain twist;

[0008] Finally, the carbon nanotube yarn, or the carbon nanotube yarn and ordinary yarn are woven into carbon nanotube yarn woven fabric through automated knitting technology.

[0009] in:

[0010] The floating catalytic chemical vapor deposition method is used to prepare carbon nanotube fibers. An organic solvent such as ethanol is used as a carbon source, ferrocene is used as a catalyst, and thiophene is used as a co-catalyst. The three together form a carbon source precursor liquid. The carbon source precursor liquid is injected into a tubular furnace, and in a carrier gas atmosphere of hydrogen and argon, carbon nanotube aerogel is catalyzed to form, and carbon nanotube fibers are obtained after water shrinkage and drying.

[0011] Furthermore, in the carbon source precursor solution, the mass ratio of ethanol ranges from 80wt% to 98wt%, preferably from 85wt% to 98wt%; the mass ratio of ferrocene ranges from 0.1wt% to 4.0wt%, preferably from 1.0wt% to 3.5wt%; the mass ratio of thiophene ranges from 0.1wt% to 4.0wt%, preferably from 1.0wt% to 3.5wt%; the sum of the three satisfies 100wt%.

[0012] The carbon nanotube fiber has a diameter of 20-80 μm, preferably 30-50 μm.

[0013] The carbon nanotube yarn has a diameter of 40-200 μm, preferably 60-150 μm, and a twist of 500-4000, preferably 1000-3500. The carbon nanotube yarn can be further twisted to obtain a carbon nanotube twisted yarn, the carbon nanotube twisted yarn has a diameter of 80-1000 μm, preferably 100-800 μm, and a twist of 350-3000, preferably 700-2000.

[0014] The twisting direction of the carbon nanotube yarn is Z direction or S direction.

[0015] The structure of the carbon nanotube knitted fabric is one of a plain weft needle, a double-sided plain weft needle, a rib, and a double rib structure.

[0016] The common yarn is one or more of polyester yarn, aramid yarn, acrylic yarn, nylon yarn and spandex yarn.

[0017] The carbon nanotube yarn braid prepared by the present invention has an average electromagnetic shielding of more than 30 dB in the X-band (8.2-12.4 GHz), and has good electromagnetic shielding application prospects.

[0018] The beneficial effects of the present invention are:

[0019] (1) We achieved the continuous and synchronous twisting of carbon nanotube fibers into carbon nanotube yarns, and used automated knitting technology to prepare carbon nanotube yarn woven fabrics with various structures.

[0020] (2) The prepared carbon nanotube yarn woven fabric has good flexibility and electromagnetic shielding performance, and is expected to be used in various fields such as flexible electronic materials, aerospace, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is an optical photo of carbon nanotube fiber.

[0022] Figure 2 Optical photograph of carbon nanotube yarn.

[0023] Figure 3 Schematic diagram of carbon nanotube yarn weaving fabric.

[0024] Figure 4 Optical photos and scanning electron microscope photos of double-sided weft plain knitted fabrics made of carbon nanotube yarn and their electromagnetic shielding effectiveness.

[0025] Figure 5 Optical photos and scanning electron microscope photos of carbon nanotube yarn double rib fabric and its electromagnetic shielding effectiveness.

[0026] Figure 6 Optical photos and scanning electron microscope photos of carbon nanotube / aramid yarn double-sided plain needle tuck fabric and its electromagnetic shielding effectiveness. DETAILED DESCRIPTION

[0027] The present invention is further described below by way of embodiments in conjunction with the accompanying drawings.

[0028] The experimental methods without specific conditions in the examples are carried out according to conventional methods and conditions, or according to the product specifications. Room temperature refers to an ambient temperature of 10-30°C.

[0029] Example 1: Preparation and testing of carbon nanotube yarn braids

[0030] Step (1): Preparation of carbon nanotube fibers

[0031] In a floating catalytic reactor, ferrocene is used as a catalyst, thiophene is used as a co-catalyst, and ethanol is used as a carbon source to form a carbon source precursor solution, and the mass ratio of the three is 2.5wt% / 2.5wt% / 95wt%. The carbon source precursor solution is continuously injected into a quartz tube through a peristaltic pump. At a reaction temperature of 1250°C, argon is used as a carrier gas with a flow rate of 100mL / min, and hydrogen is used as a reducing gas with a flow rate of 1400mL / min. Carbon nanotube aerogels are continuously obtained. After water shrinkage and densification, carbon nanotube fibers ( Figure 1 ).

[0032] Step (2): Preparation of carbon nanotube yarn

[0033] The carbon nanotube fibers prepared in step (1) are continuously twisted by a synchronous twisting device to obtain a 4-in-1 carbon nanotube yarn ( Figure 2 ), where the twist is set to 1500 and the twisting direction is the Z direction.

[0034] Step (3): Preparation of carbon nanotube yarn woven fabric

[0035] The carbon nanotube yarn obtained in step (2) is woven by an automated knitting device to obtain a carbon nanotube yarn woven fabric with a double-sided plain weft needle structure ( Figure 3 ).

[0036] The electromagnetic shielding test of this fabric was carried out using a vector network analyzer in the X-band (8.2-12.4GHz), and the average electromagnetic shielding effectiveness of the fabric was found to be 34dB, of which the average reflection effectiveness was 8.5dB and the average absorption effectiveness was 25.5dB ( Figure 4 ).

[0037] Example 2: Preparation and testing of carbon nanotube yarn braids

[0038] Step (1): Preparation of carbon nanotube fibers;

[0039] As described in Example 1.

[0040] Step (2): Preparation of carbon nanotube yarn;

[0041] As described in Example 1.

[0042] Step (3): preparing carbon nanotube yarn blended knitted fabric;

[0043] The carbon nanotube yarn obtained in step (2) is woven by an automatic knitting device to obtain a carbon nanotube material with a double rib structure.

[0044] The electromagnetic shielding test of this fabric was carried out using a vector network analyzer in the X-band (8.2-12.4GHz), and the average electromagnetic shielding effectiveness of the fabric was found to be 19.0dB, of which the average reflection effectiveness was 7.0dB and the average absorption effectiveness was 12.0dB ( Figure 5 ).

[0045] Example 3: Preparation and testing of carbon nanotube yarn braids

[0046] Step (1): Preparation of carbon nanotube fibers

[0047] As described in Example 1.

[0048] Step (2): Preparation of carbon nanotube yarn

[0049] As described in Example 1.

[0050] Step (3): Preparation of carbon nanotube yarn blended knitted fabric

[0051] The carbon nanotube yarn and aramid yarn obtained in step (2) are put into an automated knitting device together to weave a carbon nanotube / aramid blended fabric with a double-sided plain weft needle tuck structure.

[0052] The electromagnetic shielding test of this fabric was carried out using a vector network analyzer in the X-band (8.2-12.4GHz), and the average electromagnetic shielding effectiveness of the fabric was found to be 37.3dB, of which the average reflection effectiveness was 9.6dB and the average absorption effectiveness was 27.7dB ( Figure 6)。

Claims

1. A method for preparing a carbon nanotube yarn braid with electromagnetic shielding function, characterized in that: The specific steps are: (1) Preparing carbon nanotube fibers using floating catalytic chemical vapor deposition; (2) continuously combining and twisting a plurality of carbon nanotube fibers into a carbon nanotube yarn having a certain twist; (3) Weaving carbon nanotube yarn, or carbon nanotube yarn and ordinary yarn into carbon nanotube yarn woven fabric through automated knitting technology.

2. The preparation method according to claim 1, characterized in that: The floating catalytic chemical vapor deposition method for preparing carbon nanotube fibers in step (1) specifically comprises: using ethanol organic solvent as a carbon source, ferrocene as a catalyst, and thiophene as a co-catalyst, the three of which constitute a carbon source precursor liquid; after the carbon source precursor liquid is injected into a tubular furnace, it is catalytically formed into carbon nanotube aerogel in a carrier gas atmosphere of hydrogen and argon, and the carbon nanotube fibers are obtained after water shrinkage and drying.

3. The preparation method according to claim 2, characterized in that: In the carbon source precursor solution, the mass ratio of ethanol is in the range of 80wt%-98wt%, the mass ratio of ferrocene is in the range of 0.1wt%-4.0wt%, and the mass ratio of thiophene is in the range of 0.1wt%-4.0wt%, and the total of the three satisfies 100wt%.

4. The preparation method according to claim 1, characterized in that: The diameter of the carbon nanotube fiber in step (1) is 20-80 μm.

5. The preparation method according to claim 1, characterized in that: In step (2), the diameter of the carbon nanotube yarn is 40-200 μm, and the twist is 500-4000. The yarn diameter is controlled by the number of twisted carbon nanotube fibers and the yarn twist.

6. The preparation method according to claim 5, characterized in that: In step (2), the carbon nanotube yarn is further paralleled and twisted into a carbon nanotube complex twisted yarn with a diameter of 80-1000 μm and a twist of 350-3000. The diameter of the complex twisted yarn is controlled by the number of paralleled carbon nanotube yarns and the complex twist twist.

7. The preparation method according to claim 1, characterized in that: The twisting direction of the carbon nanotube yarn is Z direction or S direction.

8. The preparation method according to claim 1, characterized in that: Step (3) The structure of the carbon nanotube yarn woven fabric is one of plain weft needle, double-sided plain weft needle, double-sided plain weft needle tuck, rib, and double rib.

9. The preparation method according to claim 1, characterized in that: The common yarn is one or more of polyester yarn, aramid yarn, acrylic yarn, nylon yarn and spandex yarn.

10. A carbon nanotube yarn braid with electromagnetic shielding function obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Carbon nano tube fiber knitted fabric and preparation method thereof

    CN108301109A

  • Carbon nanotube composite yarn and preparation method thereof

    CN113089149A

  • Carbon nanotube twisted yarn, and method for producing the same

    JP2011153392A

  • Catalysts for the large scale production of high purity carbon nanotubes with chemical vapor deposition

    WO2006087590A1