Method for manufacturing regenerated leather by using chromium leather scrap fiber dry method
Through multi-point chemical crosslinking modification technology, the Schiff base reaction is carried out using PEI and GA solutions to enhance the tangle effect of chromium leather chip collagen fibers, and the collagen fiber hot melt bonding denaturation and chromium ion dechromium in the prior art are solved. The problem of detanning achieves high strength and uniformity of recycled leather and avoids environmental pollution.
Patent Information
- Application Number
- CN202410979195.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing dry preparation technology of recycled leather, the mixed melt bonding of collagen fibers leads to denaturation, the adhesive has weak force, which affects physical properties, and when alkaline substances are used to adjust the pH value, chromium ions are dechromatized and detanned, resulting in Environmental pollution.
Using multi-point chemical crosslinking modification method, polyethyleneimine (PEI) and glutaraldehyde (GA) are used as modifiers and crosslinking agents to enhance the tangle of collagen fibers through Schiff base reaction and avoid alkaline Use of sexual substances to prepare chromium leather chip fiber dry regeneration leather.
It improves the physical strength and uniformity of the recycled leather, avoids the escape and oxidation of heavy metal chromium, maintains the natural characteristics of collagen fibers, and has good mechanical properties and safety of the product.
Smart Images

Figure CN118932600A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the fields of resource utilization technology of leather waste and regenerated leather processing technology, and in particular to a method for dry-processing regenerated leather by utilizing chrome leather scrap fibers. Background Art
[0002] While the tanning industry brings economic benefits to economic development, the large amount of leather scraps it produces has put tremendous pressure on the ecological environment. Among them, leather scraps mainly include: trimming scraps, gray leather pieces, shavings and other wastes before tanning; leather shavings, trimmings and other chromium-containing scraps after chrome tanning. Among the leather scraps, most are chromium-containing scraps. Traditional methods of leather scrap treatment mainly include incineration and landfilling. The treatment process is relatively extensive, resulting in a huge waste of protein resources; at the same time, the chromium in leather scraps poses a serious threat to the ecological environment.
[0003] Regenerated leather manufacturing is an important way to achieve large-scale recycling of chrome-containing leather scraps. Commonly used methods for preparing regenerated leather include wet method and dry method. The wet method was a commonly used method for preparing regenerated leather in the early days. It mainly involves hydraulically pulping the chrome leather scraps, adding a series of additives such as adhesives, laying the mesh to form, squeezing water and drying, and finishing to obtain sheet regenerated leather. However, the wet production process often has disadvantages such as high water consumption, easy agglomeration and entanglement of the slurry, complex production process, many types of auxiliary agents required and large amounts, and easy to produce secondary pollution.
[0004] At present, there are relatively few publicly reported patents on dry-process preparation technology for regenerated leather. Among them, the Chinese patent "CN1137305 C Dry-process Production of Regenerated Leather" discloses a method for manufacturing regenerated leather. Regenerated leather is prepared by stripping leather fibers, adding and mixing thermosetting fibers, and then needle punching and hot melt bonding.
[0005] Chinese patent "CN 103088503 B Method for Modifying Collagen Fiber Bundles" discloses a method for preparing fiber raw materials by modifying collagen fiber bundles with an aqueous adhesive and then drying and opening the fibers.
[0006] Chinese patent "CN 114164680 B A method for preparing durable antibacterial and mildew-proof regenerated leather and its application" discloses a method for preparing regenerated leather by immersing composite leather fibers in an antibacterial aqueous polyurethane solution.
[0007] Chinese patent "CN 105835494 B Heat storage and temperature regulating regenerated leather and its preparation method" discloses a method for preparing heat storage and temperature regulating regenerated leather by adding aqueous polyurethane emulsion and heat storage microcapsules.
[0008] Chinese patent "CN 102864581 B A method for manufacturing a breathable genuine leather fiber flocking base fabric" discloses a method of using waste leather crushed and mixed with oxidized starch, and using hot pressing technology to enhance the composite between collagen fibers. This method changes the conventional process of using resin and other adhesives, and at the same time mixes plant fibers to make the obtained base fabric have good breathability and physical strength.
[0009] However, the technical solutions disclosed in the above Chinese patent documents still have many technical disadvantages or limitations, including:
[0010] (1) Chinese patent "CN 1137305 C Dry process for producing regenerated leather" uses heat-cured fiber mixed with collagen fibers to be hot-melt bonded at 170°C. Under these conditions, the collagen fibers are denatured, which seriously affects the product performance.
[0011] (2) The technologies reported in the Chinese patents “CN 103088503 B Modification method of collagen fiber bundles”, “CN 114164680B Preparation method and application of durable antibacterial and mildew-proof regenerated leather”, “CN 105835494 B Heat storage and temperature regulating regenerated leather and its preparation method”, and the paper “Exploration of wet properties of glued regenerated leather prepared by dry method” all use adhesives such as polyurethane. The adhesive is used to bond collagen fibers to achieve material molding under dry pressing. In this method, there is no covalent bond between the adhesive and the collagen fibers, and the component interaction force is very weak, which affects the improvement of physical properties. This defect is more obvious for powdered fibers less than 3 mm. Increasing the amount of adhesive can alleviate this problem, but it will result in too low a proportion of collagen fibers, causing the regenerated leather to lose its natural characteristics.
[0012] (3) Chinese patent "CN 102864581 B A method for manufacturing a breathable genuine leather fiber flocking base cloth" changes the conventional process of using adhesives, mixes crushed waste leather with oxidized starch, causes the two to undergo a Schiff base reaction, and enhances the entanglement and bonding effect between the fibers. The reactivity of oxidized starch is very low. In order to induce a reaction between waste leather and oxidized starch, the technology uses soda ash to adjust the pH value of the mixed system to 6-8. However, it should be pointed out that: 1. Adjusting the pH value of chromium-containing waste leather scraps from less than 4 to 6-8 requires a large amount of soda ash. More seriously, during the process of increasing pH, the metal chromium ions in the chromium waste leather scraps that were originally firmly bound to the collagen fibers will gradually lose their binding force with the carboxyl groups of the collagen fibers (i.e., dechrome detanning phenomenon), become free, and cause serious secondary pollution. Some trivalent chromium ions may even be oxidized by oxygen in the air in the presence of alkaline substances to become highly toxic hexavalent chromium, which will remain in the recycled leather products or exist in wastewater, poisoning the environment and affecting the physical and mental health of operators and the safe use of products. 2. Oxidized starch is a large-scale granular substance. After mixing with leather collagen fibers, it cannot be evenly distributed. After heating, the particles melt, and the area that interacts with the collagen fibers is limited to the periphery of the molten particles, which undoubtedly affects the uniformity of the product and limits the physical properties.
[0013] Therefore, in the preparation of dry-process regenerated leather, when processing regenerated leather products mainly composed of collagen fibers, how to avoid using adhesives and instead utilize multi-point chemical cross-linking modification methods to enhance the cross-linking density and entanglement between collagen fibers is a research topic with very positive and practical significance. In addition, how to avoid the use of alkaline substances, prevent the escape and oxidation of heavy metal chromium, and improve product uniformity are also research topics with very positive and practical significance. Summary of the invention
[0014] In view of this, the purpose of the present invention is to propose a method for dry-processing regenerated leather using chrome leather scraps fibers, which is reliable to implement, flexible to apply and fully utilizes the cross-linking and entanglement between raw materials to enhance the structural strength of the regenerated leather.
[0015] In order to achieve the above technical objectives, the technical solution adopted by the present invention is:
[0016] A method for producing regenerated leather by dry process using chrome leather scraps fiber, comprising:
[0017] After the chrome leather shavings collagen fibers are combed, they are pressed into collagen fiber mats, and then immersed in PEI solution to allow the PEI solution to penetrate into the collagen fiber mats. GA solution is then added to react for a preset time to allow the aldehyde groups of GA in the GA solution to react with the amino groups of PEI in the PEI solution and the amino groups of collagen in the collagen fiber mats to undergo Schiff base reactions, thereby generating multi-point cross-linking between collagen and PEI to modify and enhance the entanglement and bonding between the chrome leather shavings collagen fibers. Finally, the collagen fiber mats are taken out for dehydration, drying and hot pressing to obtain regenerated leather.
[0018] As a possible implementation manner, further, the chrome leather shavings collagen fibers described in this solution are combed by a fiber combing machine, and the number of combing times is 2 to 8 times.
[0019] As a preferred implementation option, preferably, the combed chrome leather shavings collagen fibers of this solution are spread in a container covered with non-woven fabric and pressed into collagen fiber mats.
[0020] As a possible implementation manner, further, the length of the chrome leather shavings collagen fibers described in this solution is 1 to 4 mm.
[0021] As a preferred implementation option, preferably, the mass concentration of the PEI solution in this scheme is 2% to 10% (w / v), which is prepared by dissolving PEI in water.
[0022] As a preferred implementation option, preferably, the mass concentration of the GA solution described in this scheme is 0.25% to 1.5% (w / v), which is prepared by dissolving GA in water.
[0023] As a preferred implementation option, preferably, the collagen fiber mat described in this scheme is immersed in the PEI solution for 30 to 90 minutes, and then the GA solution is added to react for 30 to 70 minutes.
[0024] As a preferred implementation option, preferably, the volume ratio of the PEI solution to the GA solution in this solution is 5-15:3-10.
[0025] As a preferred implementation option, preferably, the collagen fiber mat of this scheme is dehydrated to a dripping state by physical method, placed in a vacuum drying environment of 53-97°C for 5-20 minutes, and then transferred to a hot press for hot pressing at working parameters of 60-100°C and 1-3MPa for 10-30 minutes.
[0026] Based on the above, the present invention also provides a regenerated leather, which is prepared by the above method.
[0027] By adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art:
[0028] 1. This scheme does not use adhesives when manufacturing recycled leather. Instead, it uses the characteristics that the active amino groups in the collagen molecular chains in the chrome-containing leather scraps are not occupied by chromium coordination. The polyamino compound PEI is used as a modifier and glutaraldehyde is used as a binary cross-linking agent. The entanglement between collagen fibers is effectively enhanced through a one-step multi-point chemical cross-linking modification method, so that the product has good physical strength;
[0029] 2. The main component of the regenerated leather product in this scheme is collagen fiber, which maintains the genuine leather feel of the regenerated product;
[0030] 3. This solution avoids the use of alkaline substances during the processing process, and avoids the escape and oxidation of heavy metal chromium;
[0031] 4. The polyethyleneimine and glutaraldehyde used in this scheme have good water solubility and can quickly and evenly penetrate the collagen fibers, ensuring the uniformity of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0033] Figure 1 The SEM characterization image of the regenerated leather prepared in Example 3 of this scheme and the SEM image of the regenerated leather directly prepared from pure chrome leather scraps collagen fibers in the control group, wherein: Figure 1 (a) is the SEM characterization image of the control group 1, which is made of regenerated leather made of pure chrome leather scraps collagen fibers. Figure 1 (b) Microscopic representation of the regenerated leather obtained in Example 3;
[0034] Figure 2 This is a comparison chart of tensile stress detection of the regenerated leather produced in Example 3 of this scheme and the regenerated leather produced in other parallel examples. DETAILED DESCRIPTION
[0035] The present invention will be further described in detail below in conjunction with the accompanying drawings and examples. It is particularly noted that the following examples are only used to illustrate the present invention, but are not intended to limit the scope of the present invention. Similarly, the following examples are only partial embodiments of the present invention rather than all embodiments, and all other embodiments obtained by those of ordinary skill in the art without creative work are within the scope of protection of the present invention.
[0036] The PEI solution used in the embodiment of this scheme is obtained by dissolving PEI (polyethyleneimine, molecular weight 1800) in deionized water, and the GA solution used is obtained by dissolving GA (glutaraldehyde) in deionized water; the chrome leather shavings collagen fibers used are 1 to 4 mm in length.
[0037] Example 1
[0038] The present embodiment provides a method for producing regenerated leather by dry process using chrome leather scraps fiber, which comprises:
[0039] 15g of chrome leather shavings collagen fibers were combed twice by a fiber combing machine until they were in a loose state, and then spread on a container covered with non-woven fabric for physical pressing into a collagen fiber mat. The collagen fiber mat was then immersed in 150ml of a 3.2% (w / v) PEI solution for 30 minutes to allow the PEI solution to penetrate into the collagen fiber mat, and then 100ml of a 1.5% (w / v) GA solution was added to react for 40 minutes. After the reaction was completed, the collagen fiber mat was taken out for physical dehydration until it did not drip, and then placed at 64°C for vacuum drying for 15 minutes, and then transferred to a hot press and hot pressed at 60°C and 1MPa for 30 minutes to obtain regenerated leather.
[0040] Example 2
[0041] The present embodiment provides a method for producing regenerated leather by dry process using chrome leather scraps fiber, which comprises:
[0042] 15g of chrome leather shavings collagen fibers were combed 8 times by a fiber combing machine until they were in a loose state, and then spread on a container covered with non-woven fabric for physical pressing into a collagen fiber mat. The collagen fiber mat was then immersed in 50ml of a 10% (w / v) PEI solution for 60 minutes to allow the PEI solution to penetrate into the collagen fiber mat, and then 100ml of a 0.5% (w / v) GA solution was added to react for 50 minutes. After the reaction was completed, the collagen fiber mat was taken out for physical dehydration until it did not drip, and then placed at a temperature of 53°C for vacuum drying for 10 minutes, and then transferred to a hot press and hot pressed at 80°C and 3MPa for 20 minutes to obtain regenerated leather.
[0043] Example 3
[0044] The present embodiment provides a method for producing regenerated leather by dry process using chrome leather scraps fiber, which comprises:
[0045] 15g of chrome leather shavings collagen fibers were combed 5 times by a fiber combing machine until they were in a loose state, and then spread on a container covered with non-woven fabric for physical pressing into a collagen fiber mat. The collagen fiber mat was then immersed in 150ml of a 3.2% (w / v) PEI solution for 60 minutes to allow the PEI solution to penetrate into the collagen fiber mat, and then 100ml of a 0.75% (w / v) GA solution was added to react for 60 minutes. After the reaction was completed, the collagen fiber mat was taken out for physical dehydration until it did not drip, and then placed at 97°C for vacuum drying for 5 minutes, and then transferred to a hot press and hot pressed at 90°C and 2MPa for 10 minutes to obtain regenerated leather.
[0046] For the convenience of comparison, this example also directly heat-presses pure chrome leather scraps collagen fibers using the same heat-pressing parameters as above to make regenerated leather as control group 1; then SEM characterization is performed on them respectively to explore the microscopic differences. The results are as follows Figure 1 As shown. Among them, Figure 1 (b) shows the microstructure morphology of the regenerated leather made from chrome leather shavings collagen fibers after PEI / GA coordinated modification in this embodiment, which reflects that the PEI / glutaraldehyde coordinated modification makes the surface of the chrome leather shavings collagen fibers covered with PEI components, and compared with the pure chrome leather shavings collagen fibers ( Figure 1 The fibers of the regenerated leather material formed by (a)) are more tightly entangled and cohesive.
[0047] In addition, this embodiment also constructs a control group 2 (prepared sample B) in which PEI is not added, only GA is added, and other parameters are the same; a control group 3 (prepared sample C) in which PEI is added, GA is not added, and other parameters are the same, and the tensile stress is compared with the sample A prepared by the combined modification of PEI and GA. The results are as follows: Figure 2 As shown, it can be seen that the regenerated leather made from chrome leather shavings collagen fibers modified jointly by PEI and GA has good mechanical strength (maximum tensile stress can reach 6.6 MPa), which is much higher than the values of PEI modification alone or GA modification alone, proving that there is a significant synergistic effect between PEI and GA in the preparation of regenerated leather.
[0048] Therefore, it can be seen from the test results that this scheme uses polyethyleneimine and glutaraldehyde to synergistically modify the amino-rich chrome leather shavings collagen fibers for use as regenerated leather, which improves the disadvantage that the collagen fibers are too short to be conducive to dry molding, enhances the entanglement and bonding between the fibers, and then performs hot pressing molding to obtain a regenerated leather product with a compact structure and good mechanical strength.
[0049] Example 4
[0050] The present embodiment provides a method for producing regenerated leather by dry process using chrome leather scraps fiber, which comprises:
[0051] 15g of chrome leather shavings collagen fibers were combed 4 times by a fiber combing machine until they were in a loose state, and then spread on a container covered with non-woven fabric for physical pressing into a collagen fiber mat. The collagen fiber mat was then immersed in 100ml of a 6% (w / v) PEI solution for 40 minutes to allow the PEI solution to penetrate into the collagen fiber mat, and then 60ml of a 1% (w / v) GA solution was added to react for 30 minutes. After the reaction was completed, the collagen fiber mat was taken out for physical dehydration until it did not drip, and then placed at 86°C for vacuum drying for 5 minutes, and then transferred to a hot press and hot pressed for 15 minutes at a hot pressing parameter of 100°C and 1MPa to obtain regenerated leather.
[0052] Example 5
[0053] The present embodiment provides a method for producing regenerated leather by dry process using chrome leather scraps fiber, which comprises:
[0054] 15g of chrome leather shavings collagen fibers were combed twice by a fiber combing machine until they were in a loose state, and then spread on a container covered with non-woven fabric for physical pressing into a collagen fiber mat. The collagen fiber mat was then immersed in 75ml of a 4% (w / v) PEI solution for 90 minutes to allow the PEI solution to penetrate into the collagen fiber mat, and then 100ml of a 1% (w / v) GA solution was added to react for 70 minutes. After the reaction was completed, the collagen fiber mat was taken out for physical dehydration until it did not drip, and then placed at 75°C for vacuum drying for 20 minutes, and then transferred to a hot press and hot pressed at 70°C and 2MPa for 10 minutes to obtain regenerated leather.
[0055] The above descriptions are only some embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Any equivalent device or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for producing regenerated leather by dry process using chrome leather scraps fiber, characterized in that: It includes: After the chrome leather shavings collagen fibers are combed, they are pressed into collagen fiber mats, and then immersed in PEI solution to allow the PEI solution to penetrate into the collagen fiber mats. GA solution is then added to react for a preset time to allow the aldehyde groups of GA in the GA solution to react with the amino groups of PEI in the PEI solution and the amino groups of collagen in the collagen fiber mats to undergo Schiff base reactions, thereby generating multi-point cross-linking between collagen and PEI to modify and enhance the entanglement and bonding between the chrome leather shavings collagen fibers. Finally, the collagen fiber mats are taken out for dehydration, drying and hot pressing to obtain regenerated leather.
2. The method for producing regenerated leather by dry process using chrome leather scraps fiber according to claim 1, characterized in that: The chrome leather scraps collagen fibers are combed by a fiber combing machine, and the number of combing times is 2 to 8 times.
3. The method for producing regenerated leather by dry process using chrome leather scraps fiber as claimed in claim 2, characterized in that: The combed chrome leather shavings collagen fibers are spread in a container covered with non-woven fabrics and pressed into collagen fiber mats.
4. The method for producing regenerated leather by dry process using chrome leather scraps fiber as claimed in claim 1, characterized in that: The length of the chrome leather shavings collagen fibers is 1 to 4 mm.
5. The method for producing regenerated leather by dry process using chrome leather scraps fiber according to any one of claims 1 to 4, characterized in that: The mass concentration of the PEI solution is 2% to 10% (w / v), and is prepared by dissolving PEI in water.
6. The method for producing regenerated leather by dry process using chrome leather scraps fiber as claimed in claim 5, characterized in that: The mass concentration of the GA solution is 0.25% to 1.5% (w / v), and is prepared by dissolving GA in water.
7. The method for producing regenerated leather by dry process using chrome leather scraps fiber as claimed in claim 6, characterized in that: The collagen fiber mat is immersed in the PEI solution for 30 to 90 minutes, and then the GA solution is added to react for 30 to 70 minutes.
8. The method for producing regenerated leather by dry process using chrome leather scraps fiber as claimed in claim 7, characterized in that: The added volume ratio of the PEI solution to the GA solution is 5-15:3-10.
9. The method for producing regenerated leather by dry process using chrome leather scraps fiber as claimed in claim 7, characterized in that: The collagen fiber mat is physically dehydrated to a drip-free state, and then placed in a vacuum drying environment at 53-97° C. for 5-20 min. It is then transferred to a hot press and hot pressed for 10-30 min at working parameters of 60-100° C. and 1-3 MPa.
10. A regenerated leather, characterized in that: It is prepared by the method according to any one of claims 1 to 9.