Preparation method of nano-zinc oxide sanitary napkin antibacterial composite fiber mesh fabric

By using nano zinc oxide powder and composite fiber technology, the problems of sanitary napkins' antibacterial performance are not lasting and water absorption are insufficient, and efficient antibacterial, improved mechanical properties and breathability are achieved, and the comfort and safety of use are improved.

CN118932698APending Publication Date: 2024-11-12PINGXIANG XIAORI TECH CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410898799.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The antibacterial properties of existing sanitary napkins are not long-lasting enough and are easily affected by the environment and use conditions. The addition of antibacterial agents may lead to reduced skin irritation and water absorption, insufficient breathability, and affect user comfort and health.

Method used

Using nano zinc oxide powder with particle size of 10-50nm, antibacterial agent is prepared by ultrasonic treatment and pH control, combined with composite natural fibers and synthetic fibers, and pulsed electric field treatment is used to make nano zinc oxide antibacterial agent evenly adhere to the fiber mesh surface. Form an antibacterial composite fiber mesh surface.

Benefits of technology

It significantly improves the antibacterial effect and durability of sanitary napkins, improves mechanical properties and breathability, improves water absorption and comfort, while reducing irritation and environmental impact on the skin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004929884650000071
    Figure BDA0004929884650000071
  • Figure BDA0004929884650000072
    Figure BDA0004929884650000072
  • Figure BDA0004929884650000081
    Figure BDA0004929884650000081
Patent Text Reader

Abstract

The invention provides a preparation method of a nano-zinc oxide sanitary napkin antibacterial composite fiber mesh fabric, which comprises the following steps: dispersing nano-zinc oxide powder in a dispersion liquid with a specific ratio, and carrying out ultrasonic treatment and pH adjustment to obtain a uniform antibacterial agent; the preparation method comprises the following steps: mixing natural fibers and synthetic fibers, treating by using a spinning aid, preparing a fiber mesh base material by using spinning and weaving processes, firmly attaching an antibacterial agent to the fiber mesh base material by using a pulsed electric field technology, and finally, cutting, sewing and packaging to prepare the nano-zinc oxide sanitary napkin with excellent performance. The broad-spectrum antibacterial property of the nano zinc oxide is utilized, so that the antibacterial effect of the sanitary towel is remarkably improved. Meanwhile, due to the optimized design of the composite fibers, the mechanical performance of the fiber mesh surface is enhanced, the air permeability and the water absorption are improved, the antibacterial effect of the sanitary towel is ensured, meanwhile, the comfort and the use convenience are also considered, and a safe, comfortable and efficient new product choice is provided for the sanitary towel market.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sanitary products, and in particular to a method for preparing an antibacterial composite fiber mesh fabric of a nano zinc oxide sanitary napkin. Background Art

[0002] With the improvement of people's living standards and the enhancement of health awareness, the demand for personal hygiene products, especially sanitary napkins, is increasing. As a necessity in women's daily life, sanitary napkins have antibacterial properties, mechanical properties, breathability, water absorption and other properties that directly affect the comfort and health of users.

[0003] In the prior art, the antibacterial treatment of sanitary napkins mainly relies on adding antibacterial agents or using antibacterial fabrics. However, these methods have many shortcomings. On the one hand, the amount of antibacterial agents added and the way they are used are often difficult to control. Excessive use may cause skin irritation or allergies, and uneven addition of antibacterial agents may lead to decreased antibacterial performance. On the other hand, the antibacterial effect of traditional antibacterial fabrics is not long-lasting and is easily affected by the environment and usage conditions. Nano zinc oxide has broad-spectrum antibacterial properties, but the addition of nano zinc oxide may have a certain effect on the softness, water absorption and air permeability of the fiber mesh. How to ensure the uniform distribution, stability and long-term effectiveness of nano zinc oxide on the fiber mesh still requires further research and optimization.

[0004] In addition, some sanitary napkins may sacrifice breathability in pursuit of good water absorption, causing users to feel damp and uncomfortable, which may have an adverse effect on women's health in the long run. The mechanical properties, breathability and water absorption of sanitary napkins are also key factors that restrict their performance. Existing sanitary napkins often have problems with mechanical properties such as deformation and breakage after long-term use. At the same time, poor breathability and insufficient water absorption also affect the user's comfort experience. Therefore, how to maintain or improve the comfort of the fabric while ensuring the antibacterial effect is a problem that needs to be solved. Summary of the invention

[0005] In view of this, the present invention proposes a method for preparing an antibacterial composite fiber mesh fabric of a nano zinc oxide sanitary napkin to solve the above problems.

[0006] The technical solution of the present invention is achieved as follows: a method for preparing an antibacterial composite fiber mesh fabric of a nano zinc oxide sanitary napkin: comprising the following steps: first preparing a nano zinc oxide antibacterial agent, then preparing a fiber mesh base material, then uniformly dispersing the nano zinc oxide antibacterial agent and impregnating the fiber mesh base material to form an antibacterial composite fiber mesh, and finally performing post-processing to meet the use requirements of the sanitary napkin product.

[0007] Furthermore, a method for preparing a nano zinc oxide sanitary napkin antibacterial composite fiber mesh fabric comprises the following steps:

[0008] S1. Select nano zinc oxide powder with a particle size of 10-50 nm, add it to the dispersion, the mass volume ratio of the nano zinc oxide powder to the dispersion is 12-20:25 g / mL, use ultrasonic treatment to fully dissolve or disperse it, adjust the pH value to 9-10, and obtain a nano zinc oxide antibacterial agent with a mass concentration of 0.5-2%;

[0009] S2, using a composite natural fiber and a synthetic fiber mixed, soaking in a spinning aid, controlling the soaking temperature to 20-30°C, the soaking time to 12-24h, the pH to 7-9, and extruding the obtained spinning solution through a spinneret, and making a fiber mesh base material through spinning, braiding or weaving processes;

[0010] S3, immersing the nano zinc oxide antibacterial agent in the dispersion of the nano zinc oxide antibacterial agent, treating it with constant temperature oscillation for 40-80 minutes, and intermittently performing pulse electric field treatment for 5-8 times, each time for 30-60 seconds, with an interval of 3-8 minutes, and drying and curing at 80-120° C. after the treatment, so that the nano zinc oxide antibacterial agent is firmly attached to the fiber mesh surface to form an antibacterial composite fiber mesh surface;

[0011] S4, cutting, sewing and packaging the mesh surface to make nano zinc oxide sanitary napkins.

[0012] Furthermore, the dispersion of S1 comprises the following raw materials in parts by weight: 80-90 parts of ethanol, 1-5 parts of polymethyl methacrylate, and 1-5 parts of hexadecyltrimethylammonium bromide.

[0013] Furthermore, the ultrasonic frequency of S1 is 50-60kHz, and the ultrasonic power is 2.2-3.5kW / m 2 , ultrasonic treatment for 25-55min.

[0014] Furthermore, the mixing mass ratio of the natural fiber and the synthetic fiber in S2 is 8-10:1.

[0015] Furthermore, the composite natural fiber of S2 includes cotton fiber, silk fiber, grapefruit silk fiber and corn fiber in a mass ratio of (10-30):(12-33):(6-9):(2-5).

[0016] Furthermore, the synthetic fiber of S2 includes any one of polypropylene fiber, polyethylene fiber, polyester fiber, and acrylic polymer.

[0017] Furthermore, the spinning aid of S2 comprises the following raw materials in parts by weight: 10-12 parts of N-methylmorpholine-N-oxide, 3-8 parts of urea, 1-3 parts of coconut shell oil, and 0.3-1.5 parts of 1,1,3,3-tetramethylguanidine methoxyacetate.

[0018] Furthermore, the constant temperature oscillation treatment temperature of S3 is 55-85° C., and the oscillation frequency is 3000-3800 rpm.

[0019] Furthermore, the S3 pulse electric field strength is 18-33 kV / cm, the frequency is 100-225 Hz, and the pulse width is 25-38 μS.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) Highly effective antibacterial performance: The antibacterial effect of sanitary napkins is significantly improved by using nano zinc oxide powder with a particle size of 10-50nm. Nano zinc oxide can effectively inhibit the growth of a variety of bacteria and fungi and reduce the risk of infection due to its high specific surface area and strong antibacterial activity. In addition, ultrasonic treatment and precise control of pH value ensure the uniform dispersion of the antibacterial agent in the dispersion, further improving the durability and extensiveness of the antibacterial effect. At the same time, pulse electric field treatment is intermittently performed under oscillating conditions, so that the nano zinc oxide antibacterial agent can be evenly and firmly attached to the fiber mesh surface and is not easy to fall off. This not only ensures the durability of the antibacterial effect, but also avoids the potential irritation of the antibacterial agent to the skin during use.

[0022] (2) Improved mechanical properties: This method uses a mixture of composite natural fibers and synthetic fibers, combining the softness and comfort of natural fibers with the high strength of synthetic fibers, so that the sanitary napkins remain soft and comfortable while also having better durability and tensile resistance. This fiber combination provides the sanitary napkin with balanced mechanical properties, ensuring stable performance under different use conditions. And soaking in a specific spinning aid can reduce and improve the uniformity and continuity of the fibers, further improve the liquid absorption rate and water retention capacity of the sanitary napkin and improve the mechanical properties of the fiber mesh.

[0023] (3) Optimized air permeability: Through the carefully designed fiber mesh structure and spinning process, this method optimizes the air permeability of the sanitary napkin. The dispersion of nano zinc oxide particles will not hinder air circulation. At the same time, the selection of composite fibers and the weaving process further improve the air permeability of the fabric, which helps to reduce moisture accumulation, keep the skin dry and reduce discomfort.

[0024] (4) Improved water absorption: The natural fibers selected in this method have good water absorption. Combined with the treatment of nano zinc oxide antimicrobial agent, not only does it not reduce the water absorption capacity of the sanitary napkin, but it also improves the absorption and diffusion efficiency of the liquid through the optimized fiber structure and surface treatment. This enables the sanitary napkin to quickly absorb and lock in liquid, reduce the risk of leakage, and provide longer-term comfort.

[0025] (5) Environmental protection and safety: The nano zinc oxide used in this method is a safe and environmentally friendly antibacterial agent. Compared with traditional chemical antibacterial agents, it reduces the potential impact on the environment and irritation to the human body. At the same time, through pulsed electric field treatment, the use of high temperature or harmful chemicals is avoided, ensuring the safety and environmental protection of the product. DETAILED DESCRIPTION

[0026] In order to better understand the technical content of the present invention, specific embodiments are provided below to further illustrate the present invention.

[0027] Unless otherwise specified, the experimental methods used in the embodiments of the present invention are all conventional methods.

[0028] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources.

[0029] Example 1

[0030] A method for preparing an antibacterial composite fiber mesh fabric of a nano zinc oxide sanitary napkin comprises the following steps:

[0031] S1. Select nano zinc oxide powder with a particle size of 10 nm and add it to a dispersion. The dispersion includes the following raw materials in parts by weight: 80 parts of ethanol, 1 part of polymethyl methacrylate, and 1 part of hexadecyltrimethylammonium bromide. The mass volume ratio of nano zinc oxide powder to dispersion is 12:25 g / mL. Ultrasonic treatment is used to fully dissolve or disperse it. The ultrasonic frequency is 50 kHz and the ultrasonic power is 2.2 kW / m 2 , ultrasonic treatment for 25 min, adjusting the pH value to 9, and obtaining a nano zinc oxide antibacterial agent with a mass concentration of 0.5%;

[0032] S2, using composite natural fiber and synthetic fiber mixed in a mass ratio of 8:1, the composite natural fiber includes cotton fiber, silk fiber, grapefruit silk fiber, corn fiber in a mass ratio of 10:12:6:2, and the synthetic fiber includes polypropylene fiber, soaked in a spinning aid, the spinning aid includes the following raw materials in parts by weight: 10 parts of N-methylmorpholine-N-oxide, 3 parts of urea, 1 part of coconut shell oil, 0.3 parts of 1,1,3,3-tetramethylguanidine methoxyacetate, the soaking temperature is controlled at 20°C, the soaking time is 12h, the pH is 7, the obtained spinning solution is extruded through a spinneret, and a fiber mesh base material is made by spinning, braiding or weaving process;

[0033] S3, immersing the nano zinc oxide antibacterial agent in the dispersion of the nano zinc oxide antibacterial agent, treating it at a constant temperature of 55°C and an oscillation frequency of 3000rpm for 40min, and intermittently performing a pulse electric field treatment for 5 times, each time for 30s, with an interval of 3min, the pulse electric field strength is 18kV / cm, the frequency is 100Hz, and the pulse width is 25μS. After the treatment, drying and curing is performed at 80°C to make the nano zinc oxide antibacterial agent firmly adhere to the fiber mesh surface to form an antibacterial composite fiber mesh surface;

[0034] S4, cutting, sewing and packaging the mesh surface to make nano zinc oxide sanitary napkins.

[0035] Example 2

[0036] A method for preparing an antibacterial composite fiber mesh fabric of a nano zinc oxide sanitary napkin comprises the following steps:

[0037] S1. Select nano zinc oxide powder with a particle size of 50 nm and add it to a dispersion. The dispersion includes the following raw materials in parts by weight: 90 parts of ethanol, 5 parts of polymethyl methacrylate, and 5 parts of hexadecyltrimethylammonium bromide. The mass volume ratio of nano zinc oxide powder to dispersion is 20:25 g / mL. Ultrasonic treatment is used to fully dissolve or disperse it. The ultrasonic frequency is 60 kHz and the ultrasonic power is 3.5 kW / m 2 , ultrasonic treatment for 55 min, adjusting the pH value to 10, and obtaining a nano zinc oxide antibacterial agent with a mass concentration of 2%;

[0038] S2, using composite natural fiber and synthetic fiber in a mass ratio of 10:1, the composite natural fiber includes cotton fiber, silk fiber, grapefruit silk fiber, corn fiber in a mass ratio of 30:33:9:5, and the synthetic fiber is polyethylene fiber, soaked in a spinning aid, the spinning aid includes the following raw materials in parts by weight: 12 parts of N-methylmorpholine-N-oxide, 8 parts of urea, 3 parts of coconut shell oil, 1.5 parts of 1,1,3,3-tetramethylguanidine methoxyacetate, the soaking temperature is controlled at 30°C, the soaking time is 24h, the pH is 9, the obtained spinning solution is extruded through a spinneret, and a fiber mesh base material is made by spinning, braiding or weaving process;

[0039] S3, immersing the nano zinc oxide antibacterial agent in the dispersion of the nano zinc oxide antibacterial agent, treating it at a constant temperature of 85°C and an oscillation frequency of 3800rpm for 80min, and intermittently performing a pulse electric field treatment for 8 times, each time for 60s, with an interval of 8min, the pulse electric field strength is 33kV / cm, the frequency is 225Hz, and the pulse width is 38μS. After the treatment, it is dried and cured at 120°C to make the nano zinc oxide antibacterial agent firmly adhere to the fiber mesh surface to form an antibacterial composite fiber mesh surface;

[0040] S4, cutting, sewing and packaging the mesh surface to make nano zinc oxide sanitary napkins.

[0041] Example 3

[0042] A method for preparing an antibacterial composite fiber mesh fabric of a nano zinc oxide sanitary napkin comprises the following steps:

[0043] S1. Select nano zinc oxide powder with a particle size of 30 nm and add it to a dispersion. The dispersion includes the following raw materials in parts by weight: 85 parts of ethanol, 3 parts of polymethyl methacrylate, and 3 parts of hexadecyltrimethylammonium bromide. The mass volume ratio of nano zinc oxide powder to dispersion is 16:25 g / mL. Ultrasonic treatment is used to fully dissolve or disperse it. The ultrasonic frequency is 55 kHz and the ultrasonic power is 2.8 kW / m 2 , ultrasonic treatment for 40 min, adjusting the pH value to 9, and obtaining a nano zinc oxide antibacterial agent with a mass concentration of 1.5%;

[0044] S2, using composite natural fiber and synthetic fiber in a mass ratio of 9:1, the composite natural fiber includes cotton fiber, silk fiber, grapefruit silk fiber, corn fiber in a mass ratio of 20:25:7:3, and the synthetic fiber is polyethylene fiber, soaked in a spinning aid, the spinning aid includes the following raw materials in parts by weight: 11 parts of N-methylmorpholine-N-oxide, 5 parts of urea, 2 parts of coconut shell oil, 0.9 parts of 1,1,3,3-tetramethylguanidine methoxyacetate, the soaking temperature is controlled at 25°C, the soaking time is 18h, the pH is 8, the obtained spinning solution is extruded through a spinneret, and a fiber mesh base material is made by spinning, braiding or weaving process;

[0045] S3, immersing the nano zinc oxide antibacterial agent in the dispersion of the nano zinc oxide antibacterial agent, treating it with constant temperature oscillation at a temperature of 70°C and an oscillation frequency of 3500rpm for 60min, and intermittently performing pulse electric field treatment 7 times, each time for 45s, with an interval of 5min, the pulse electric field strength is 25kV / cm, the frequency is 160Hz, and the pulse width is 31μS. After the treatment, drying and curing is performed at 100°C to make the nano zinc oxide antibacterial agent firmly adhere to the fiber mesh surface to form an antibacterial composite fiber mesh surface;

[0046] S4, cutting, sewing and packaging the mesh surface to make nano zinc oxide sanitary napkins.

[0047] Comparative Example 1

[0048] The difference between this comparative example and Example 3 is that the sanitary napkin fabric does not contain nano zinc oxide antibacterial agent.

[0049] Comparative Example 2

[0050] The difference between this comparative example and Example 3 is that, in the method for preparing the sanitary napkin fabric, in the step S2, during the mixing process of the composite natural fiber and the synthetic fiber, the fabric is not immersed in a spinning aid, but in an ethanol solution with a mass concentration of 77%.

[0051] Comparative Example 3

[0052] The difference between this comparative example and Example 3 is that, in the preparation method of the sanitary napkin fabric, the pulse electric field treatment is not performed discontinuously in the S3 step; specifically, the nano zinc oxide antibacterial agent is immersed in the dispersion of the nano zinc oxide antibacterial agent, and the treatment is performed at a constant temperature and oscillation for 60 minutes. After the treatment, the nano zinc oxide antibacterial agent is dried and solidified at 100°C, so that the nano zinc oxide antibacterial agent is firmly attached to the fiber mesh surface to form an antibacterial composite fiber mesh surface.

[0053] 1. Effect Verification

[0054] The sanitary napkin fabrics prepared in Examples 1-3 of the present invention and Comparative Examples 1-3 were subjected to mechanical property tests, antibacterial tests, water absorption tests, and air permeability tests. The specific tests are as follows:

[0055] (1) Mechanical properties tests include softness and breaking strength tests;

[0056] a. Softness: Tested in accordance with GB / T 8942-2016;

[0057] b. Breaking strength test: Tested in accordance with GB / T 3923.1-2013;

[0058] The test results are shown in Table 1:

[0059]

[0060] (2) Antibacterial test: Three groups of bacterial suspensions were added to the above Examples 1-3 and Comparative Examples 1-3 and commercially available sanitary napkins, and each group was tested 3 times on average. The exposure time was 15 hours, and the cells were placed in a 37°C incubator for 48 hours. The number of live bacterial colonies was observed and recorded. The bacterial suspensions were Staphylococcus aureus, Escherichia coli, and Candida albicans.

[0061] The calculation formula of the antibacterial rate is: X = (AB) / A × 100%,

[0062] Where X is the inhibition rate, A is the average colony count of the control sample, and B is the average colony count of the tested sample;

[0063] The test results are shown in Table 2 below:

[0064]

[0065] (3) Water absorption test: Under a pressure of 2 kPa, 100 mL of liquid was poured onto the sanitary napkin fabrics prepared in the above Examples 1-3 and Comparative Examples 1-3 and commercially available sanitary napkins, and the time required for complete absorption was tested;

[0066] (4) Air permeability test: Determination of air permeability of fabrics according to GB / T5453-1997;

[0067] The results are shown in Table 3:

[0068]

[0069] Combined with the results in Tables 1-3 above, it can be seen that compared with commercially available sanitary napkins, the sanitary napkin fabric prepared by the present invention has better antibacterial properties, softness, breaking strength, water absorption and air permeability; softness ≤10.9mN, transverse breaking strength ≥42.3N, longitudinal breaking strength ≥98.1N, Staphylococcus aureus inhibition rate reaches 100%, Escherichia coli inhibition rate ≥99.8%, Candida albicans ≥99.7%; distilled water absorption time ≤4.2s, physiological saline absorption time ≤4.9s, physiological saline containing 10g hemoglobin absorption time ≤9.2s; air permeability 592-598mm / s.

[0070] Comparison between Example 3 and Comparative Example 1 shows that the use of nano zinc oxide powder, utilizing its unique nano effect, can effectively inhibit the growth and reproduction of bacteria.

[0071] By comparing Example 3 with Comparative Example 2, the method of mixing composite natural fibers and synthetic fibers in a specific ratio can combine the advantages of both, and form a fiber mesh with a porous structure, optimize the microstructure of the fiber, facilitate air circulation, improve the air permeability of the sanitary napkin, reduce humidity and stuffiness, and soak in a specific spinning aid, and control the soaking temperature and time, so as to obtain a more uniform and stable spinning solution. This helps to improve the uniformity and continuity of the fiber, further improve the liquid absorption speed and water retention capacity of the sanitary napkin, and improve the mechanical properties of the fiber mesh;

[0072] By comparing Example 3 with Comparative Example 3, intermittent pulse electric field treatment is performed on the rice zinc oxide antibacterial agent during immersion in the dispersion of the nano zinc oxide antibacterial agent, thereby enhancing the binding force between the nano zinc oxide antibacterial agent and the fiber mesh surface, ensuring the durability and uniform distribution of the antibacterial agent, so that the addition of the nano zinc oxide antibacterial agent will not significantly affect the water absorption performance of the fiber mesh surface, and at the same time its antibacterial properties help to keep the surface of the sanitary napkin dry and clean.

[0073] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a nano zinc oxide sanitary napkin antibacterial composite fiber mesh fabric, Features: The following steps are involved: First, a nano zinc oxide antibacterial agent is prepared, and then a fiber mesh base material is prepared. The nano zinc oxide antibacterial agent is evenly dispersed and impregnated on the fiber mesh base material to form an antibacterial composite fiber mesh. Finally, post-treatment is performed to meet the use requirements of sanitary napkin products.

2. A method for preparing the antibacterial composite fiber mesh fabric of a nano zinc oxide sanitary napkin as claimed in claim 1, Features: The following steps are involved: S1, select nano zinc oxide powder with a particle size of 10-50nm, add it to the dispersion, the mass volume ratio of nano zinc oxide powder to dispersion is 12-20 g / mL:

25. Use ultrasonic treatment to fully dissolve or disperse it, adjust the pH value to 9-10, and obtain a nano zinc oxide antibacterial agent with a mass concentration of 0.5-2%; S2, using a composite natural fiber and a synthetic fiber mixed, soaking in a spinning aid, controlling the soaking temperature to 20-30°C, the soaking time to 12-24h, the pH to 7-9, and extruding the obtained spinning solution through a spinneret, and making a fiber mesh base material through spinning, braiding or weaving processes; S3, immersing the nano zinc oxide antibacterial agent in the dispersion of the nano zinc oxide antibacterial agent, treating it with constant temperature oscillation for 40-80 minutes, and intermittently performing pulse electric field treatment for 5-8 times, each time for 30-60 seconds, with an interval of 3-8 minutes, and drying and curing at 80-120° C. after the treatment, so that the nano zinc oxide antibacterial agent is firmly attached to the fiber mesh surface to form an antibacterial composite fiber mesh surface; S4, cutting, sewing and packaging the mesh surface to make nano zinc oxide sanitary napkins.

3. A method for preparing the antibacterial composite fiber mesh fabric of a nano zinc oxide sanitary napkin as claimed in claim 2, Features: The dispersion of S1 comprises the following raw materials in parts by weight: 80-90 parts of ethanol, 1-5 parts of polymethyl methacrylate, and 1-5 parts of hexadecyltrimethylammonium bromide.

4. A method for preparing the antibacterial composite fiber mesh fabric of a nano zinc oxide sanitary napkin as claimed in claim 2, Features: The ultrasonic frequency of S1 is 50-60kHz, and the ultrasonic power is 2.2-3.5kW / m 2 , ultrasonic treatment for 25-55min.

5. The method for preparing the antibacterial composite fiber mesh fabric of a nano zinc oxide sanitary napkin as claimed in claim 2, Features: The mixing mass ratio of the natural fiber and the synthetic fiber in S2 is 8-10:

1.

6. A method for preparing the antibacterial composite fiber mesh fabric of a nano zinc oxide sanitary napkin as claimed in claim 2, Features: The composite natural fiber of S2 includes cotton fiber, silk fiber, grapefruit silk fiber and corn fiber in a mass ratio of (10-30):(12-33):(6-9):(2-5).

7. A method for preparing the antibacterial composite fiber mesh fabric of a nano zinc oxide sanitary napkin as claimed in claim 2, Features: The synthetic fiber of S2 includes any one of polypropylene fiber, polyethylene fiber, polyester fiber, and acrylic polymer.

8. The method for preparing the antibacterial composite fiber mesh fabric of a nano zinc oxide sanitary napkin as claimed in claim 2, Features: The spinning aid of S2 comprises the following raw materials in parts by weight: 10-12 parts of N-methylmorpholine-N-oxide, 3-8 parts of urea, 1-3 parts of coconut shell oil, and 0.3-1.5 parts of 1,1,3,3-tetramethylguanidine methoxyacetate.

9. The method for preparing the antibacterial composite fiber mesh fabric of a nano zinc oxide sanitary napkin as claimed in claim 2, Features: The constant temperature oscillation treatment temperature of S3 is 55-85° C., and the oscillation frequency is 3000-3800 rpm.

10. The method for preparing the antibacterial composite fiber mesh fabric of a nano zinc oxide sanitary napkin as claimed in claim 2, Features: The S3 pulse electric field strength is 18-33 kV / cm, the frequency is 100-225 Hz, and the pulse width is 25-38 μS.

Citation Information

Cited By

  • Absorber of novel environment-friendly composite fiber sanitary towel as well as preparation method and application

    CN120360781A

  • Nano-zinc oxide modified antibacterial fiber and preparation method thereof

    CN120519985A

  • Antibacterial moisture-absorbing breathable sanitary towel and preparation method thereof