Preparation method of moisture-absorbing and heating silk fiber

By swelling, laser etching, ultrasonic cleaning and grafting reactions on silk fibers, and combining sand washing and finishing to form a velvet structure, the problem of easy fall off of hygroscopic heating finishing agent is solved, and the durability and effect of hygroscopic heating performance is significantly improved.

CN118932709APending Publication Date: 2024-11-12SHANGHAI SHUIXING HOME TEXTILE CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411155581.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Among the existing hygroscopic heat-generating silk products, the hygroscopic heat-generating finishing agent is prone to fall off, resulting in the hygroscopic heat-generating performance being not lasting, and the fuzz structure caused by sand washing and finishing cannot effectively adhere to the hygroscopic heat-generating finishing agent.

Method used

The silk fibers were swelled in 1-ethyl-3-methylimidazole acetate solution and laser etching was carried out to form a microstructure. Then, hydrophilic groups were introduced through ultrasonic cleaning and grafting reaction, and finally sand washing and finishing to form The velvet structure ensures even adhesion of the hygroscopic heating finisher.

Benefits of technology

The performance durability and hygroscopic heating fibers are improved, and the microstructure is closed by the villi structure to prevent the finishing agent from falling off, and the adhesion amount and distribution uniformity of the hygroscopic heating agent are increased.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of textile fibers. A preparation method of moisture-absorbing and heating silk fibers comprises the following steps: step 1, soaking and swelling silk fibers to obtain swollen fibers; step 2, performing laser etching on the swollen fibers to obtain microporous fibers; 3, hydrophilic groups are introduced into the microporous fibers through a grafting reaction, and grafted fibers are obtained; step 4, carrying out sand washing finishing on the branch fibers to obtain fluff fibers; step 5, performing moisture-absorbing and heating finishing on the fluff fibers to obtain the moisture-absorbing and heating fibers. The moisture absorption and heating effect of the moisture absorption and heating fiber obtained by the invention is far higher than that of the moisture absorption and heating fiber obtained by the technology in the background technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textile fibers, and in particular to a method for preparing textile fibers. Background Art

[0002] The patent application with application number CN2020110786730 and patent name "A method for preparing modified grafted hygroscopic and heat-generating silk" provides a method for preparing hygroscopic and heat-generating silk. The method first modifies and grafts the silk fibers, then performs hygroscopic and heat-generating finishing, and finally performs sand washing finishing.

[0003] Although natural silk products are endowed with the function of absorbing moisture and generating heat, the hygroscopic and heat-generating finishing is done by immersion, and the hygroscopic and heat-generating finishing agent only acts on the surface of the silk and is easy to fall off. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing moisture-absorbing and heat-generating silk fibers to solve the above-mentioned technical problems.

[0005] The technical problem solved by the present invention can be achieved by adopting the following technical solutions:

[0006] A method for preparing moisture-absorbing and heat-generating silk fiber comprises the following steps:

[0007] Step 1, soaking the silk fiber in a 1-ethyl-3-methylimidazolium acetate solution to swell the silk fiber, thereby obtaining swollen fiber;

[0008] Step 2, laser etching the swollen fiber to form a microstructure on its surface to obtain microporous fiber;

[0009] Step 3, after ultrasonic cleaning of the microporous fiber in clean water, leaving it to dry, and then introducing hydrophilic groups through a grafting reaction to obtain a grafted fiber;

[0010] Step 4, sand washing the grafted fibers to form a fluff structure on the surface of the grafted fibers to obtain fluff fibers;

[0011] Step 5: Perform moisture absorption and heat generation finishing on the fluff fibers to obtain moisture absorption and heat generation fibers.

[0012] Effective effects:

[0013] 1. The hygroscopic and heat-generating fiber obtained by the present invention has a hygroscopic and heat-generating finishing agent not only attached to the outer surface of the fiber, but also attached to the microstructure and villi structure of the fiber. Therefore, the hygroscopic and heat-generating effect is much higher than that of the hygroscopic and heat-generating fiber obtained by the technology in the background technology.

[0014] 2. The hygroscopic and heat-generating fiber obtained by the present invention has a closed microstructure by means of a fluff structure, so that the hygroscopic and heat-generating finishing agent in the microstructure is not easy to fall off, thereby improving the durability of the hygroscopic and heat-generating performance.

[0015] 3. The present invention first performs sand washing and then performs hygroscopic and heat-generating finishing. Compared with the method of first performing hygroscopic and heat-generating finishing and then performing sand washing in the background technology, on the one hand, it can solve the problem of hygroscopic and heat-generating finishing agent falling off caused by sand washing, and on the other hand, it can make the fluff structure produced by sand washing also adhere to the hygroscopic and heat-generating finishing agent, thereby increasing the amount of hygroscopic and heat-generating finishing agent, and then improving the hygroscopic and heat-generating performance.

[0016] 4. Compared with the technology in the background art, the present invention adds a laser etching step, and forms a microstructure on the silk fiber by laser etching. The microstructure is used to increase the reaction area of ​​the grafting reaction and accommodate the hygroscopic and heat-generating finishing agent.

[0017] 5. Compared with the technology in the background art, the present invention has an additional swelling step, which can greatly improve the uniformity of the laser-etched microstructure, thereby making the hygroscopic and heat-generating finishing agent more evenly distributed.

[0018] Preferably, a method for preparing hygroscopic heat-generating silk fiber further comprises step 6, using common fiber as the core yarn and hygroscopic heat-generating fiber as the decorative yarn, feeding the core yarn and the decorative yarn into an air-changing device, the feeding roller speed of the decorative yarn is greater than the feeding roller speed of the core yarn, and the overfeed ratio is 5-6 times, and the core yarn and the decorative yarn are interwoven and entangled together in the air-changing device to form a composite fiber, thereby improving the performance of the common fiber.

[0019] Preferably, after step 1 and before step 2, the swollen fiber is flattened and drained for 5 to 10 minutes to allow the suspension solution to naturally detach under gravity, which helps to protect the swollen fiber structure; setting the draining time at 5 to 10 minutes helps the batch of swollen fibers to tend to a homogenized state, which not only maintains a certain humidity, but also ensures that the suspension solution tends to fall completely; then, in the flattened state, blow with 50 to 80 degrees Celsius hot air from bottom to top for 3 to 5 seconds; blow dry with hot air from bottom to top, at least offset most of the gravity on the downward aggregation of the liquid, so that the overall humidity of the swollen fiber is uniform; blow with 50 to 80 degrees Celsius hot air for 3 to 5 seconds; protect the swollen fiber from high temperature damage, and provide a sufficiently high temperature, so that the evaporation of the swollen fiber surface is much greater than that of the swollen fiber depth. Make the surface of the swollen fiber tend to dry, but retain the solution moisture in the deep swollen fiber, which provides technical conditions for controlling the etching depth during laser etching and ensuring the strength of the swollen fiber. Because the surface of the swollen fiber tends to dry but the solution moisture is retained inside, laser etching occurs on the surface of the swollen fiber, protecting the deep structure of the swollen fiber. In this way, the laser etching microstructure of the swollen fiber surface is obtained while ensuring the fiber strength.

[0020] The laser etching method is as follows: the swollen fiber layer is laid on a stage, the ambient humidity is set to 80%-90%, the ambient temperature is set to 25°C-30°C, the laser power is 3W-5W, the laser etching speed is 1500mm / s, and the etching is repeated 2-3 times. Based on the water retention deep in the swollen fiber in the steps of the present invention, the laser power is allowed to be larger, set to 3W-5W, which can improve the processing efficiency and greatly improve the laser etching quality of the surface layer.

[0021] Preferably, water retaining plates are arranged around the stage, a first notch is formed on the water retaining plate on one side of the stage, a second notch is formed on the water retaining plate on the other side opposite to the stage, and the height of the top surface of the stage gradually increases from the first notch to the second notch; the swollen fiber enters from the first notch and then exits from the second notch, and the 1-ethyl-3-methylimidazole acetate solution moves along the stage toward the first notch and flows out through the first notch, thereby collecting the 1-ethyl-3-methylimidazole acetate solution.

[0022] Preferably, the silk is tussah silk, and the silk is subjected to moisture absorption and heat generation finishing by soaking in finishing liquid, wherein the finishing liquid contains a moisture absorption and heat generation finishing agent and a softener, so as to improve the performance of the tussah silk. DETAILED DESCRIPTION

[0023] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below.

[0024] A method for preparing moisture-absorbing and heat-generating silk fiber comprises the following steps:

[0025] Step 1, soaking and swelling the silk fiber in a 1-ethyl-3-methylimidazolium acetate solution to obtain swollen fiber. The 1-ethyl-3-methylimidazolium acetate solution is preferably a 1-ethyl-3-methylimidazolium acetate solution with a mass concentration of 5%. The soaking time is preferably 20 minutes. First, the volume of the swollen fiber becomes larger, so that the microstructure formed by the laser etching in the next step is more uniform. Secondly, the hydrogen bonds of the swollen fiber grow, and there are sufficient space and chemical sites for subsequent grafting reactions. In the process of soaking and swelling, it is preferred to vibrate the 1-ethyl-3-methylimidazolium acetate solution using ultrasound. Ultrasonic vibration can accelerate the swelling rate of silk fibers on the one hand, thereby reducing the soaking time; on the other hand, it can separate silk fibers from each other. The present invention selects the type and concentration of the swelling solution. 1-ethyl-3-methylimidazolium acetate is very hygroscopic, so the trace amount of 1-ethyl-3-methylimidazolium acetate remaining on the silk fiber can effectively increase the hygroscopicity of the silk fiber. More importantly, it is incompatible with strong oxidants, which can reduce the requirements for the selection and proportion of strong oxidants in subsequent sand washing and finishing.

[0026] Step 2: laser etching the swollen fiber to form a microstructure on its surface to obtain microporous fiber.

[0027] After the swollen fiber is flattened, drain for 5 to 10 minutes to allow the suspension solution to naturally detach under gravity, which helps to protect the swollen fiber structure; setting the drain time at 5 to 10 minutes helps the batch of swollen fibers to tend to a homogenized state, which not only maintains the same humidity, but also ensures that the suspension solution tends to fall completely; then, in the flattened state, blow with 50 to 80 degrees Celsius hot air from bottom to top for 3 to 5 seconds; blow dry with hot air from bottom to top, at least offset most of the gravity on the downward aggregation of the liquid, so that the overall humidity of the swollen fiber is uniform; blow with 50 to 80 degrees Celsius hot air for 3 to 5 seconds; protect the swollen fiber from high temperature damage, and provide a high enough temperature, so that the evaporation of the swollen fiber surface is much greater than that of the swollen fiber deep. Make the surface of the swollen fiber tend to dry, but retain the solution moisture in the deep swollen fiber, which provides technical conditions for controlling the etching depth during laser etching and ensuring the strength of the swollen fiber. Because the surface of the swollen fiber tends to dry, but the solution moisture is retained inside, laser etching occurs on the surface of the swollen fiber, protecting the deep structure of the swollen fiber, thereby obtaining the laser-etched microstructure of the swollen fiber surface and ensuring the fiber strength. The 1-ethyl-3-methylimidazolium acetate solution contained in the swollen fiber plays a role in protecting the silk fiber during the laser etching process, which can prevent the temperature at the silk fiber from being too high, thereby allowing the laser etching speed to increase. At the same time, the 1-ethyl-3-methylimidazolium acetate solution contained in the swollen fiber plays a role in isolating the silk fibers from each other, making the laying more uniform, thereby making the etched microstructure more uniform, and the silk fibers are not easy to break, thereby allowing the number of repeated etching to be increased.

[0028] The laser etching method is as follows: the swollen fiber layer is spread on a stage, the ambient humidity is set to 80%-90%, the ambient temperature is set to 25°C-30°C, the laser power is 3W-5W, the laser etching speed is 1500mm / s, and the etching is repeated 2-3 times. Preferably, the swollen fiber in step (1) is subjected to the following treatment before being placed on the stage. Based on the water retention deep in the swollen fiber in the steps of the present invention, the laser power is allowed to be larger and set to 3W-5W, which can improve the processing efficiency and greatly improve the laser etching quality of the surface layer.

[0029] During the laser etching process, part of the 1-ethyl-3-methylimidazole acetate solution flows out from the microporous fiber. A water retaining plate can be set around the stage to prevent the 1-ethyl-3-methylimidazole acetate solution from flowing everywhere. Preferably, a first notch is provided on the water retaining plate on one side of the stage, and a second notch is provided on the water retaining plate on the other side opposite to the stage, and the height of the top surface of the stage gradually increases from the first notch to the second notch. The swollen fiber enters from the first notch and then exits from the second notch. The 1-ethyl-3-methylimidazole acetate solution moves along the stage toward the first notch. A collecting tank is provided below the first notch. After passing through the first notch, the 1-ethyl-3-methylimidazole acetate solution falls into the collecting tank below, thereby collecting the 1-ethyl-3-methylimidazole acetate solution.

[0030] Step 3, after ultrasonic cleaning of the microporous fiber in clean water, let it stand to dry, and then introduce hydrophilic groups through grafting reaction to obtain grafted fiber. Clean water ultrasonic cleaning can be carried out first to effectively remove 1-ethyl-3-methylimidazole acetate, open the microstructure, and improve the effect of subsequent grafting reaction. Preferably, the grafting reaction can be carried out by soaking the microporous fiber in the reaction solution. The functional solution preferably contains 5% polyacrylonitrile (owf). Preferably, the temperature is 55℃-60℃, the bath ratio is 10:1-20:1, and the soaking is for half an hour.

[0031] Step 4: sand-wash the grafted fiber to form a fluff structure on the grafted fiber surface to obtain fluff fiber. On the one hand, the fluff is used to seal the micropores, increase the grafting reaction time and the subsequent hygroscopic and exothermic finishing agent content. On the other hand, the fluff structure can increase the contact area with the hygroscopic and exothermic finishing agent and improve the hygroscopic and exothermic effect. On the other hand, the fluff structure can increase the capillary structure of the fiber and improve the water absorption effect.

[0032] Step 5, subjecting the fluff fiber to hygroscopic and heat-generating finishing to obtain hygroscopic and heat-generating fiber. The hygroscopic and heat-generating fiber obtained by making mulberry silk fiber is used as hygroscopic and heat-generating mulberry silk fiber, and the hygroscopic and heat-generating fiber obtained by making tussah silk fiber is used as hygroscopic and heat-generating tussah silk fiber. The method of the present invention is particularly suitable for tussah silk fiber, and the hygroscopic performance of the tussah silk fiber treated by the present invention is not lower than that of conventional mulberry silk fiber. Preferably, it can be carried out by soaking in a finishing liquid, and the finishing liquid contains 10% (owf) of a hygroscopic and heat-generating finishing agent. Preferably, the temperature is 55°C-60°C, the bath ratio is 10:1-20:1, and the soaking is for half an hour. When treating tussah silk fiber by the method of the present invention, a softener can be added to the finishing liquid to improve the softness of tussah silk.

[0033] The present invention may further include step 6, using common fiber as core yarn and moisture-absorbing heat-generating fiber as decorative yarn, feeding the core yarn and decorative yarn into an air-changing device, wherein the feeding roller speed of the decorative yarn is greater than the feeding roller speed of the core yarn, and the overfeed ratio is 5-6 times, and the core yarn and decorative yarn are interwoven and entangled together in the air-changing device to form a composite fiber, thereby improving the performance of common fiber.

[0034] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing hygroscopic and heat-generating silk fiber, characterized in that: The steps include: Step 1, soaking the silk fiber in a 1-ethyl-3-methylimidazolium acetate solution to swell the silk fiber, thereby obtaining swollen fiber; Step 2, laser etching the swollen fiber to form a microstructure on its surface to obtain microporous fiber; Step 3, after ultrasonic cleaning of the microporous fiber in clean water, leaving it to dry, and then introducing hydrophilic groups through a grafting reaction to obtain a grafted fiber; Step 4, sand washing the grafted fibers to form a fluff structure on the surface of the grafted fibers to obtain fluff fibers; Step 5: Perform moisture absorption and heat generation finishing on the fluff fibers to obtain moisture absorption and heat generation fibers.

2. The method for preparing a moisture-absorbing and heat-generating silk fiber according to claim 1, characterized in that: The method also includes step 6, using ordinary fiber as the core yarn and hygroscopic and heat-generating fiber as the decorative yarn, feeding the core yarn and the decorative yarn into an air-changing device, wherein the feeding roller speed of the decorative yarn is greater than the feeding roller speed of the core yarn, and the overfeed ratio is 5-6 times, and the core yarn and the decorative yarn are interwoven and entangled together in the air-changing device to form a composite fiber.

3. The method for preparing a moisture-absorbing and heat-generating silk fiber according to claim 1 or 2, characterized in that: The laser etching method is as follows: spreading the swollen fiber layer on a stage, setting the ambient humidity to 80%-90%, the ambient temperature to 25°C-30°C, the laser power to 3W-5W, the laser etching speed to 1500mm / s, and repeating etching 2-3 times.

4. The method for preparing a moisture-absorbing and heat-generating silk fiber according to claim 3, characterized in that: Water retaining plates are arranged around the loading platform, a first notch is formed on the water retaining plate on one side of the loading platform, and a second notch is formed on the water retaining plate on the other side opposite to the loading platform, and the height of the top surface of the loading platform gradually increases from the first notch to the second notch; the swollen fiber enters from the first notch and then exits from the second notch, and the 1-ethyl-3-methylimidazole acetate solution moves along the loading platform toward the first notch and flows out through the first notch.

5. The method for preparing a moisture-absorbing and heat-generating silk fiber according to claim 1 or 2, characterized in that: The silk is tussah silk, which is subjected to moisture absorption and heat generation finishing by soaking in finishing liquid, wherein the finishing liquid contains a moisture absorption and heat generation finishing agent and a softener.

Citation Information

Patent Citations

  • Preparation method of modified grafted moisture-absorbing heating silk

    CN114318867A