Method for modifying carbon fibers by constructing brick-mud structural composite layer
By constructing a ‘brick-silt’ structural composite layer on the surface of the carbon fiber, the problem of insufficient interface performance of the carbon fiber composite is solved, and a high-strength and high-toughness carbon fiber composite material is achieved.
Patent Information
- Application Number
- CN202411226803.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-12
AI Technical Summary
The lack of interface performance of carbon fiber composite materials leads to a contradiction between material strength and toughness, which is difficult to improve at the same time.
By constructing a 'brick-silt' structural composite layer, a carbon film is deposited on the surface of the carbon fiber using magnetron sputtering technology, and a carbon/polydopamine composite layer with broad spectrum adhesion is formed through dopamine polymerization to enhance the carbon fiber and resin matrix. Interface bonding performance.
It realizes that carbon fiber has both high strength and high toughness, and significantly improves the interface strength between carbon fiber and resin matrix, and obtains composite materials with excellent mechanical properties.
Smart Images

Figure CN118932721A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon fiber modification, and in particular to a method for modifying carbon fiber by constructing a "brick-mud" structure composite layer. Background Art
[0002] Carbon fiber is a high-performance fiber with a carbon content of more than 90% that is transformed through solid-phase reaction of organic fibers. It has a series of excellent properties such as light weight, high strength, high modulus, and high temperature resistance. Therefore, it is used as a composite material reinforcement in aerospace, automobile and shipbuilding, wind power, photovoltaic and other fields. However, due to the smooth surface, high inertness and low surface energy of carbon fiber, it is not conducive to the infiltration and chemical bonding of resin to the fiber, resulting in more defects at the interface of carbon fiber composite materials, and stress cannot be effectively transmitted in the interface phase, thus affecting the overall performance of the composite material.
[0003] At present, the interface strength between carbon fiber and matrix resin is usually improved by eliminating surface impurities of carbon fiber, increasing fiber specific surface area, improving wettability of carbon fiber to resin matrix, introducing reactive functional groups on the material surface, and constructing interface transition zone between carbon fiber and resin, including using nanotechnology to construct multi-scale structure on the surface of carbon fiber to improve the strength and toughness of carbon fiber composites. Especially for the production of high-strength and high-toughness carbon fiber, since high strength and high toughness have always been a pair of contradictions, the improvement of material strength often sacrifices toughness. Therefore, finding a method that can effectively improve the interface performance of carbon fiber composites and simultaneously obtain carbon fiber composites with high strength and toughness has become a hot topic of concern for carbon fiber composite researchers in various countries. Summary of the invention
[0004] The purpose of the present invention is to provide a method for modifying carbon fiber by constructing a "brick-mud" structure composite layer to solve the problems existing in the above-mentioned prior art.
[0005] To achieve the above object, the present invention provides the following solutions:
[0006] One of the technical solutions of the present invention: a method for modifying carbon fiber by constructing a "brick-mud" structure composite layer, comprising the following steps: sequentially performing magnetron sputtering surface modification treatment and dopamine polymerization surface modification treatment on the carbon fiber to form a carbon / polydopamine (PDA) composite layer with a "brick-mud" structure on the surface of the carbon fiber.
[0007] Furthermore, the magnetron sputtering surface modification treatment is specifically to deposit a carbon film on the surface of the carbon fiber by magnetron sputtering.
[0008] Furthermore, the magnetron sputtering surface modification treatment uses carbon fiber as a substrate and carbon as a target.
[0009] Furthermore, the sputtering conditions of the magnetron sputtering surface modification treatment include: a vacuum degree of 2×10 -3 Pa, the target-substrate distance is 4 cm, the sputtering power is 150-450 W, the sputtering pressure is 0.8-1.5 Pa, the sputtering time is 20-50 min, high-purity argon is used as the working gas, and the argon flow rate is 20 mL / min.
[0010] Furthermore, the purity of the high-purity argon gas is 99.99%; the sputtering conditions also include: the rotation speed of the substrate holder is 30r / min.
[0011] Furthermore, the dopamine polymerization surface modification treatment includes: placing the carbon fiber that has been subjected to magnetron sputtering surface modification treatment into a dopamine solution and reacting for 6-12 hours.
[0012] Furthermore, the preparation method of the dopamine solution is: adjusting the pH value of the Tris buffer solution to 8.5, adding dopamine hydrochloride, and stirring evenly to obtain the dopamine solution.
[0013] Furthermore, the concentration of the Tris buffer solution is 0.01 mol / L; and the amount of dopamine hydrochloride added is 2 g / L.
[0014] Furthermore, the pH value of the Tris buffer solution is adjusted to 8.5 by dropping HCl solution.
[0015] Furthermore, the step of placing the carbon fiber after the surface modification by magnetron sputtering into a dopamine solution and reacting for 6-12 hours is specifically as follows: placing the carbon fiber after the surface modification by magnetron sputtering into a dopamine solution and shaking it on a shaker at room temperature for 6-12 hours. After the reaction is completed, the step of washing and drying is also included, and the drying temperature is 40° C. and the time is 24 hours.
[0016] Furthermore, the carbon fiber is pretreated before the magnetron sputtering surface modification treatment. The pretreatment specifically includes: firstly ultrasonically cleaning the carbon fiber, then soaking it in anhydrous ethanol, and finally rinsing it with water and drying it.
[0017] Furthermore, the ultrasonic cleaning is specifically ultrasonic cleaning with acetone for 24 hours; and the soaking time in anhydrous ethanol is 30 minutes.
[0018] The second technical solution of the present invention: a composite modified carbon fiber is prepared by modifying the carbon fiber according to the above method.
[0019] Furthermore, the surface of the composite modified carbon fiber is coated with a carbon / polydopamine composite layer having a "brick-mud" structure.
[0020] Technical solution three of the present invention: Application of the above-mentioned composite modified carbon fiber as a reinforcement in preparing a composite material
[0021] The fourth technical solution of the present invention is a carbon fiber / epoxy resin composite material, which uses the above-mentioned composite modified carbon fiber as a reinforcement and epoxy resin and a curing agent as a matrix.
[0022] Furthermore, the mass proportion of the composite modified carbon fiber in the carbon fiber / epoxy resin composite material is 25-40%.
[0023] Furthermore, the mass ratio of the epoxy resin to the curing agent is 100:25-30.
[0024] Many organisms in nature have formed a natural and reasonable structure after long-term natural selection, gradually achieved the unity between structure and overall mechanical properties, and showed excellent comprehensive mechanical properties. For example, the shell nacre is composed of inorganic layers and organic layers alternately stacked, the inorganic layer is mainly aragonite calcium carbonate, accounting for about 95% of the volume, and the organic layer is mainly organic protein macromolecules, accounting for about 5% of the volume. The shell nacre has a typical layered structure at different scales. At the micron scale, the shell nacre presents a three-dimensional "brick-mud" structure, with densely stacked aragonite calcium carbonate sheets as "bricks" and biopolymers as "mud" to connect the aragonite sheets. When subjected to external force loads, cracks in the surface structure are deflected at the interlayer joints, making it have higher strength and good toughness. Based on the special structure of the shell nacre, the present invention uses magnetron sputtering technology to deposit a layer of carbon film on the surface of carbon fiber, and then uses the broad-spectrum adhesion of polydopamine to construct a bionic layer structure with the "brick-mud" structural characteristics of the nacre on the surface of the carbon fiber to achieve the purpose of improving the mechanical properties of carbon fiber composites.
[0025] The reason why the present invention uses polydopamine to prepare the bionic layer structure is, on the one hand, because polydopamine has a broad spectrum of adhesion and can be modified under mild conditions; on the other hand, because polydopamine has functional groups such as hydroxyl and amino groups, it can form chemical bonds at the interface between carbon fiber and resin matrix, effectively improving the bonding performance of the composite material interface.
[0026] The present invention discloses the following technical effects:
[0027] The present invention sequentially performs magnetron sputtering surface modification treatment and dopamine polymerization surface modification treatment on carbon fiber, respectively utilizing the structural characteristics of magnetron sputtering carbon particle film layer and the adhesion characteristics of polydopamine to construct a hierarchical interface system structure with "brick-mud" characteristics on the surface of carbon fiber. The carbon / polydopamine hierarchical interface system with "brick-mud" structure enables carbon fiber to have both high strength and high toughness, and has excellent wettability to the resin matrix, which can effectively improve the interface strength between carbon fiber and matrix resin. The modified carbon fiber obtained by the composite modification method of the present invention is used as a reinforcement to prepare a composite material, and a carbon fiber composite material with high strength and toughness and excellent comprehensive mechanical properties can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 The process flow chart of the present invention for performing magnetron sputtering / PDA composite modification on carbon fiber and using the composite modified carbon fiber as a reinforcement to prepare a composite material;
[0030] Figure 2 This is a physical picture of the carbon fiber / epoxy resin composite material prepared in Application Example 1;
[0031] Figure 3 A schematic diagram of the dimensions of the carbon fiber / epoxy resin composite material prepared in Application Example 1;
[0032] Figure 4 is the X-ray diffraction pattern of carbon fiber before and after modification;
[0033] Figure 5 The infrared spectra of carbon fiber before and after modification;
[0034] Figure 6 is the SEM image of carbon fiber before and after modification, where (a 1 ) and (a 2 ) represent the surface and cross-sectional SEM images of unmodified carbon fiber (CF), (b 1 ) and (b 2 ) represent the surface and cross-sectional SEM images of carbon fiber (CF-C) after magnetron sputtering modification, (c 1 ) and (c 2 ) represent the surface and cross-sectional SEM images of carbon fibers (CF-C-PDA) after magnetron sputtering and PDA composite modification, respectively;
[0035] Figure 7 The cross-sectional SEM images of carbon fiber (CF-C) after magnetron sputtering modification and the SEM images of silicon wafers before and after modification under the same modification conditions are shown in Figure 1. 1 ) and (a 2 ) represent the cross-sectional SEM images of carbon fibers (CF-C) modified by magnetron sputtering at different magnifications, (b 1 ) and (b 2 ) represent the surface and cross-sectional SEM images of silicon wafers after magnetron sputtering modification, (c 1 ) and (c 2 ) represent the surface and cross-sectional SEM images of silicon wafers after magnetron sputtering and PDA composite modification, respectively;
[0036] Figure 8 is the atomic force microscope image of carbon fiber before and after modification, where (a 1 ) and (a 2 ) represent the surface morphology and surface roughness of unmodified carbon fiber (CF), (b 1 ) and (b 2 ) represent the surface morphology and surface roughness of carbon fiber (CF-C) after magnetron sputtering modification, (c 1 ) and (c 2 ) represent the surface morphology and surface roughness of carbon fibers (CF-C-PDA) after magnetron sputtering and PDA composite modification, respectively;
[0037] Fig. 9 Schematic diagram of the mechanism of forming a "brick-mud" structure after magnetron sputtering and PDA composite modification;
[0038] Fig.10 The contact angle (a) and surface energy (b) of carbon fiber in water and ethylene glycol before and after modification;
[0039] Fig.11 The contact angle (a) and surface energy (b) of the carbon fibers in water and ethylene glycol after being modified by dopamine polymerization for different time periods in Example 1 and Example 5;
[0040] Fig.12 It is the test dimensions and equipment schematic diagram of the interface shear test;
[0041] Fig.13 The shear strength of the carbon fiber / epoxy resin composite material prepared by using the carbon fiber before and after modification as the reinforcement in Application Example 1;
[0042] Fig.14 The shear stress-strain curve of the carbon fiber / epoxy resin composite material prepared by using the carbon fiber before and after modification as the reinforcement in Application Example 1;
[0043] Fig.15 The flexural strength of the carbon fiber / epoxy resin composite material prepared by using the carbon fiber before and after modification as the reinforcement in Application Example 1;
[0044] Fig.16 The bending stress-strain curve of the carbon fiber / epoxy resin composite material prepared by using the carbon fiber before and after modification as the reinforcement in Application Example 1;
[0045] Fig.17 The tensile strength of the carbon fiber / epoxy resin composite material prepared by using the carbon fiber before and after modification as the reinforcement in Application Example 1;
[0046] Fig.18 The tensile stress-strain curve of the carbon fiber / epoxy resin composite material prepared by using the carbon fiber before and after modification as the reinforcement in Application Example 1;
[0047] Fig.19 The optical microscope images of the tensile section of the carbon fiber / epoxy resin composite material prepared by using the carbon fiber before and after modification as the reinforcement in Application Example 1, wherein CF(a), CF-C(b), 150W(c), 250W(d), 350W(e), 450W(f) respectively represent the composite materials prepared by using CF, CF-C, CF-C-PDA-150W (prepared in Example 2), CF-C-PDA (prepared in Example 1, sputtering power 250W), CF-C-PDA-350W (prepared in Example 3), CF-C-PDA-450W (prepared in Example 4) as reinforcement;
[0048] Fig. 20 The cross-sectional SEM images of the carbon fiber / epoxy resin composite material prepared by using the carbon fiber before and after modification as the reinforcement in Application Example 1, wherein (a)-(c) respectively represent the cross-sectional SEM images of the tensile specimens of the composite material with CF, CF-C, and CF-C-PDA as the reinforcement in Example 1, and (d)-(f) respectively represent the longitudinal SEM images of the tensile specimens of the composite material with CF, CF-C, and CF-C-PDA as the reinforcement in Example 1 after fracture. DETAILED DESCRIPTION
[0049] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0050] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0051] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0052] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0053] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0054] The process flow of the present invention for performing magnetron sputtering / PDA composite modification on carbon fiber and using the composite modified carbon fiber as a reinforcement to prepare a composite material is as follows: Figure 1 shown.
[0055] The specific information of the drugs and raw materials used in the following embodiments and application examples is shown in Table 1:
[0056]
[0057]
[0058] Example 1
[0059] (1) Carbon fiber pretreatment
[0060] The cut carbon fiber unidirectional cloth was placed in an ultrasonic cleaner and ultrasonically cleaned with acetone for 24 hours to remove the sizing agent on the surface of the carbon fiber unidirectional cloth and the dust and oil attached during the processing process. The carbon fiber unidirectional cloth after ultrasonic cleaning was soaked in anhydrous ethanol for 30 minutes, and then the surface of the carbon fiber unidirectional cloth was rinsed with distilled water to ensure that there was no reagent residue on the surface. The rinsed carbon fiber unidirectional cloth was then placed in an oven for drying for later use. The pretreated carbon fiber was recorded as CF.
[0061] (2) Carbon fiber surface modification
[0062] 1) Surface modification by magnetron sputtering
[0063] A high vacuum multi-target magnetron sputtering instrument was used to deposit a carbon film on the pretreated carbon fiber unidirectional cloth. Specifically, the carbon target was mounted on the cathode plate, the carbon fiber unidirectional cloth was fixed under the substrate, and the carbon fiber unidirectional cloth was subjected to magnetron sputtering. The specific sputtering parameters were: sputtering pressure 1.0 Pa, back vacuum 2×10 -3 Pa, the target substrate distance is 4 cm, the sputtering gas is argon with a purity of 99.99%, the argon flow rate is 20 mL / min, the substrate holder rotation speed is 30 r / min, the sputtering power is 250 W, the sputtering time is 30 min, and the sample modified by magnetron sputtering is recorded as CF-C.
[0064] 2) Dopamine polymerization modification treatment (also called polydopamine modification treatment, referred to as PDA treatment)
[0065] Prepare a Tris buffer solution with a concentration of 0.01 mol / L, adjust the pH value of the buffer solution to 8.5 by dropping HCl solution, add dopamine hydrochloride to the buffer solution at a concentration of 2 g / L and stir evenly to obtain a dopamine solution. Place the carbon fiber unidirectional cloth after magnetron sputtering surface treatment in the dopamine solution, and place it on a shaker at room temperature for 9 hours to form a carbon / polydopamine composite layer with a "brick-mud" structure on the surface of the carbon fiber unidirectional cloth. The carbon fiber unidirectional cloth modified by dopamine polymerization is repeatedly washed in deionized water to remove the residual dopamine solution on the surface, and the cleaned sample is placed in a vacuum oven at 40°C and dried for 24 hours to obtain a composite modified carbon fiber. The sample after magnetron sputtering / PDA composite modification is recorded as CF-C-PDA.
[0066] Example 2
[0067] The same as Example 1, except that the sputtering power in the magnetron sputtering surface modification treatment step is 150 W, and the final product is recorded as CF-C-PDA-150W.
[0068] Example 3
[0069] The same as Example 1, except that the sputtering power in the magnetron sputtering surface modification treatment step is 350 W, and the final product is recorded as CF-C-PDA-350W.
[0070] Example 4
[0071] The same as Example 1, except that the sputtering power in the magnetron sputtering surface modification treatment step is 450 W, and the final product is recorded as CF-C-PDA-450W.
[0072] Example 5
[0073] The same as Example 1, except that the dopamine polymerization modification treatment time is 6 hours (ie, the shaking time on the shaker is 6 hours), and the final product is recorded as CF-C-PDA-6h.
[0074] Application Example 1
[0075] Preparation of carbon fiber / epoxy resin composites
[0076] Using carbon fiber unidirectional cloth before and after modification as reinforcement, epoxy resin as matrix, and a self-made mold made of polytetrafluoroethylene plate with a thickness of 1 mm, a carbon fiber / epoxy resin composite material was prepared by injection molding. The specific method is as follows: Use a cutter to cut the polytetrafluoroethylene into a hollow dumbbell-shaped structure, place the carbon fiber unidirectional cloth in the middle of the self-made mold, use double-sided tape to fix the mold up and down, and inject the epoxy resin prepared in proportion into the mold. The mass ratio of epoxy resin (JL-235) to curing agent (JH-242) is 100:27. Remove the bubbles generated in the epoxy resin and cure it at room temperature for 48 hours to obtain a carbon fiber / epoxy resin composite material, in which the mass percentage of carbon fiber in the composite material is 40%, and the mass percentage of epoxy resin in the composite material is 60%. In fact, Figure 2 As shown, the size diagram is as follows Figure 3 shown.
[0077] Six kinds of carbon fiber / epoxy resin composite materials were prepared using the unmodified carbon fiber (CF) of Example 1, the carbon fiber (CF-C) of Example 1 modified only by magnetron sputtering, and the carbon fibers of Examples 1-4 modified by magnetron sputtering (with different sputtering powers) and PDA.
[0078] Test Example 1
[0079] Structure and composition characterization
[0080] (1) Characterization of physical properties of carbon fiber (X-ray diffraction analysis)
[0081] Figure 4is the X-ray diffraction diagram of carbon fiber before and after modification, wherein CF represents the carbon fiber pretreated in Example 1, CF-C represents the carbon fiber modified only by magnetron sputtering in Example 1, and CF-C-PDA represents the carbon fiber modified by magnetron sputtering and PDA in Example 1. Figure 4 It can be seen that there are only two diffraction peaks in the XRD of carbon fiber before and after modification. One is a sharp characteristic diffraction peak at about 2θ=25°, which is the (002) plane of the typical graphite crystal structure of carbon fiber. The other is near 2θ=43°, which is a weak diffraction peak package of carbon (111), and there are no other diffraction peaks. It shows that the magnetron sputtering modification has basically no effect on the physical structure of carbon fiber. However, the peak intensity of the (002) crystal plane at about 25° has a slight change. Among the three carbon fibers, the peak intensity of the carbon fiber modified by magnetron sputtering is larger here, and the peak intensity of the carbon fiber modified by magnetron sputtering and PDA is the smallest here. This is because the graphitization degree of the selected carbon target material is relatively high. Therefore, the surface of the carbon fiber after magnetron sputtering is covered by a carbon film, and the graphitization degree of the modified carbon fiber is slightly increased. However, for the carbon fiber after the secondary modification of PDA, the intensity of the diffraction peak here is weakened, which also shows that the surface of the carbon fiber has been coated with polydopamine.
[0082] (2) Chemical structure analysis of carbon fiber surface (infrared spectrum test)
[0083] Figure 5 The infrared spectra of carbon fiber before and after modification. Figure 5 It can be seen that at 2990-2658cm -1 There are two adjacent peaks in both the modified and unmodified carbon fibers, which are derived from the CH stretching vibration peak of the carbon fibers. -1 and 1620cm -1 There are absorption peaks of OH and C=O nearby. However, by comparison, it is found that compared with the unmodified carbon fiber, the absorption peaks of OH, C=O and CH of CF-C are weakened, while the absorption peaks of OH, C=O and CH of CF-C-PDA after the second modification by PDA are enhanced. This is because the surface of the carbon fiber is covered with a layer of carbon film after being modified by magnetron sputtering. Although the film material is also composed of carbonaceous materials, there are differences between the carbonaceous structure of the target material and the carbonaceous structure of the carbon fiber, especially at 1246cm -1 The change in the characteristic peak of the CN group at 1246 cm -1The characteristic peak of CN group appears here. This is because the matrix material of carbon fiber is polyacrylonitrile, so there is CN in the carbon fiber. The characteristic CN peak of CF-C after magnetron sputtering modification basically disappears. This is because the carbon target used for sputtering is a carbonaceous material obtained by chemical vapor deposition. Therefore, the formed carbon film does not show the presence of CN group. However, CF-C-PDA after magnetron sputtering / PDA composite modification shows the characteristic CN peak here, which indicates that polydopamine is successfully deposited on the surface of carbon fiber. Magnetron sputtering cannot change the chemical groups on the surface of carbon fiber, but dopamine is rich in hydroxyl and amino groups, and it has broad-spectrum adhesion. Through self-polymerization reaction, it can form a good bond with the surface of carbon fiber, increasing the content of active groups on the surface of carbon fiber.
[0084] (3) Surface morphology characterization of carbon fiber
[0085] Scanning electron microscope (SEM) was used to observe the surface morphology of carbon fiber before and after modification. The carbon fiber was fixed on the surface of conductive glue and subjected to surface gold spraying. The magnification was set to 10K, the electron beam acceleration voltage was set to 5kV, and the working distance was about 5mm. In order to further analyze the effect of polydopamine on the morphological structure of magnetron sputtering deposited carbon film, the morphological changes of carbon film deposited on silicon wafer under the same modification conditions were compared and analyzed.
[0086] Figure 6 is the SEM image of carbon fiber before and after modification, where (a 1 ) and (a 2 ) represent the surface and cross-sectional SEM images of unmodified carbon fiber (CF), (b 1 ) and (b 2 ) represent the surface and cross-sectional SEM images of carbon fiber (CF-C) after magnetron sputtering modification, (c 1 ) and (c 2 ) represent the surface and cross-sectional SEM images of carbon fibers (CF-C-PDA) after magnetron sputtering and PDA composite modification. Figure 6 It can be seen that the surface of the untreated carbon fiber is smooth, and a carbon film structure is formed on the surface of the carbon fiber after magnetron sputtering modification, with a small number of carbon atoms aggregated together to form large particles, and an obvious microcrack structure is formed on the surface of the carbon fiber. The surface of the carbon fiber after magnetron sputtering / polydopamine composite modification still has a film-covered structure, but its granularity phenomenon is weakened, and there are attachments adhering to the fiber surface.
[0087] In order to further analyze the effect of polydopamine on the morphology of carbon films deposited by magnetron sputtering, the morphology of carbon films deposited on silicon wafers under the same modification conditions (magnetron sputtering modification + PDA modification) was compared and analyzed. Figure 7 As shown, where (a1 ) and (a 2 ) represent the cross-sectional SEM images of carbon fibers (CF-C) modified by magnetron sputtering at different magnifications, (b 1 ) and (b 2 ) represent the surface and cross-sectional SEM images of silicon wafers after magnetron sputtering modification, (c 1 ) and (c 2 ) represent the surface and cross-sectional SEM images of silicon wafers after magnetron sputtering and PDA composite modification. Figure 7 It can be seen that the magnetron sputtering carbon film deposited on the surface of carbon fiber has a typical particle stacking columnar structure, and the carbon film deposited on the silicon wafer has the same cross-sectional morphology. The carbon film deposited on the silicon wafer is composed of a combination of carbon particles with a particle size at the nanometer level, and the surface has an obvious microcrack structure. The surface of the silicon wafer after magnetron sputtering / PDA composite modification still retains a uniform particle aggregation island structure, but the microcracks between the island structures disappear. And the typical columnar structure of the cross-section of the carbon film after magnetron sputtering / PDA composite modification disappears, presenting a suspended stacking structure with uniformly distributed particles, forming a "brick-mud" spacing arrangement structure. And the cross-sectional thickness of the deposited carbon film after PDA modification increases.
[0088] Atomic force microscopy (AFM) was used to further characterize the surface morphology of carbon fibers before and after modification. Figure 8 As shown, where (a 1 ) and (a 2 ) represent the surface morphology and surface roughness of unmodified carbon fiber (CF), (b 1 ) and (b 2 ) represent the surface morphology and surface roughness of carbon fiber (CF-C) after magnetron sputtering modification, (c 1 ) and (c 2 ) represent the surface morphology and surface roughness of carbon fiber (CF-C-PDA) after magnetron sputtering and PDA composite modification. Figure 8 It can be seen that the surface of the unmodified carbon fiber (CF) is smooth with fine grooves, and the arithmetic average roughness Ra of its surface is 10.7nm. The surface of the carbon fiber (CF-C) modified by magnetron sputtering has an obvious uneven granular structure, and the roughness is significantly increased compared with the unmodified surface, and the arithmetic average roughness Ra reaches 11.3nm. The surface of CF-C-PDA modified by magnetron sputtering / PDA presents a continuous flaky stacking structure, and the surface roughness is significantly increased. The Ra value increases to 16.6nm, which is 55.14% higher than the Ra of the unmodified carbon fiber surface, which is consistent with the results shown in the SEM image. The increase in the surface roughness of the carbon fiber is conducive to the mechanical interlocking between the reinforcement and the matrix.
[0089] The carbon film deposited by magnetron sputtering is a membrane structure formed by the accumulation of carbon particles into nuclei. Therefore, not only does it have microcracks on the surface, but there are also certain pores between the particles inside the membrane layer. When the carbon fiber modified by magnetron sputtering is further modified by dopamine polymerization, dopamine and polydopamine penetrate into the pores between the accumulated carbon particles through the microcracks on the surface of the carbon film, which affects the continuous structure of the carbon film deposited by magnetron sputtering, decomposing it into a core structure and an island structure, and forming a continuous sheet-like membrane structure under the broad-spectrum adhesion of polydopamine. In addition, a "brick-mud" structure is formed between the decomposed carbon particle island structure (or core structure) and the polydopamine. The mechanism is as follows: Fig. 9 shown.
[0090] Test Example 2
[0091] Wettability analysis (dynamic contact angle test)
[0092] In order to evaluate the interfacial properties between the reinforcement and the resin matrix, the surface energy and dynamic contact angle of the carbon fiber before and after modification were characterized by a surface / interfacial tension analyzer. This test mainly uses the Wilhelmy method to obtain the contact angle of the carbon fiber in different liquids by measuring the force change. The calculation formula is shown in formula (1). The specific operation is as follows: a certain number of carbon fiber monofilaments are fixed on a cut rectangular cardboard (50mm×10mm), with a parallel spacing of 2mm between each fiber monofilament, and the length of the carbon fiber outside the fixture is kept at 6mm. The fixed carbon fiber is inserted into the test liquid, the depth threshold is 4mm, the fiber infiltration speed is 0.1mm / s, the test mass threshold is set to 0.08mg, and the advancing angle and receding angle test speed are set to 0.08mm / s.
[0093]
[0094] Where:
[0095] θ—Contact angle of carbon fiber when it moves forward in the test liquid;
[0096] d—diameter of carbon fiber monofilament;
[0097] γ—surface tension of the test liquid (mN / m);
[0098] g—gravitational acceleration, value is 9.8m / s.
[0099] The polar component and dispersion component of the carbon fiber surface energy can be calculated based on the advancing contact angle of the fiber in two test liquids of different polarities, as shown in equations (2) and (3):
[0100]
[0101] Where:
[0102] γ 1 d ——Dispersion component of the test liquid surface energy (mJ / m 2 );
[0103] γ 1 p ——Test the polar component of liquid surface energy (mJ / m 2 );
[0104] γ 1 ——Total surface energy of test liquid (mJ / m 2 );
[0105] γ f d ——Dispersion component of carbon fiber surface energy (mJ / m 2 );
[0106] γ f p ——Polar component of carbon fiber surface energy (mJ / m 2 );
[0107] γ f ——Total surface energy of carbon fiber (mJ / m 2 ).
[0108] In this experiment, deionized water was used as the polar liquid and ethylene glycol was selected as the non-polar liquid.
[0109] The interfacial properties between carbon fiber and resin matrix depend on the wettability between the two. High surface free energy can increase the wettability between fiber and resin to obtain better interfacial properties. Fig.10 are the contact angles (a) and surface energies (b) of carbon fibers in water and ethylene glycol before and after modification, wherein CF is the carbon fiber only pretreated in Example 1, CF-C is the sample modified by magnetron sputtering in Example 1, and 150W, 250W, 350W, and 450W represent CF-C-PDA prepared in Examples 1-4 at different magnetron sputtering powers. Fig.10It can be found that after surface modification, the surface contact angle of carbon fiber is reduced compared with that of unmodified carbon fiber. The contact angles of carbon fiber modified by magnetron sputtering in deionized water and ethylene glycol are reduced by 19.17% and 10.23% respectively compared with that of unmodified carbon fiber, and the surface energy of carbon fiber is increased by 33.79% compared with that of unmodified carbon fiber. The surface contact angles of carbon fiber modified by magnetron sputtering and PDA are reduced compared with that of unmodified carbon fiber in deionized water and ethylene glycol. With the increase of magnetron sputtering power, the contact angle decreases first and then increases. When the sputtering power is 250W, the contact angle is the smallest, and the reduction is the largest relative to unmodified carbon fiber, and the effect is the most significant. When the sputtering power is 250W, the contact angles of unmodified carbon fiber in deionized water and ethylene glycol are reduced by 48.9% and 55.4% respectively, and the surface energy is increased by 1.22 times compared with the surface energy of unmodified carbon fiber.
[0110] Depend on Figure 6 From the SEM images of the carbon fiber surface morphology before and after modification, it can be seen that the carbon fiber surface is relatively smooth, and the dispersion component is closely related to the surface roughness of the material, so the contact angle of the carbon fiber in ethylene glycol is relatively large. The polar component of the material surface energy is mainly related to the surface polarity of the material. Since the carbon fiber undergoes pre-oxidation, carbonization and other processes during the production process, carbon atoms are enriched on the surface of the carbon fiber, and other elements escape. The surface activity content of the carbon fiber is low, so it cannot form a good infiltration with polar solvents. Therefore, the contact angle of the carbon fiber in deionized water is large, the polar component is low, and the surface energy of the carbon fiber is also low. The contact angle of the carbon fiber surface after magnetron sputtering carbon treatment decreases because magnetron sputtering forms a carbon film structure on the surface of the carbon fiber, and the film surface has microcracks, which increases the surface roughness of the carbon fiber. Therefore, the contact angle in ethylene glycol decreases, and the microcracks on the carbon film surface play a positive role in the interaction between the carbon fiber and the liquid surface. Therefore, the contact angle in water also decreases, so the surface energy of the carbon fiber increases. After magnetron sputtering and PDA composite modification treatment, the contact angle of carbon fiber in deionized water and ethylene glycol is significantly reduced. This is because PDA reacts with carbon fiber through self-polymerization, introduces active functional groups on the surface of carbon fiber, and forms large PDA particles on the surface of carbon fiber, which reduces the polar component and dispersion component of carbon fiber, increases the surface energy of carbon fiber, and improves the wettability of carbon fiber surface, which is conducive to the possibility of further strengthening of carbon fiber and resin matrix.
[0111] Fig.11 The contact angle (a) and surface energy (b) of the carbon fibers in water and ethylene glycol after dopamine polymerization modification treatment for different time periods in Example 1 and Example 5, wherein CF-C-PDA-6h represents CF-C-PDA-6h prepared in Example 5, and CF-C-PDA-9h represents CF-C-PDA prepared in Example 1. Fig.11 Combination Fig.10It can be seen that the contact angle of the carbon fiber modified with polydopamine for 6 hours in deionized water and ethylene glycol decreased by 36.49% and 50.87% respectively compared with the unmodified carbon fiber, but it was not as obvious as the contact angle of the carbon fiber modified with polydopamine for 9 hours in deionized water and ethylene glycol. The surface energy of the carbon fiber modified with polydopamine for 6 hours increased by 79.92% compared with the unmodified carbon fiber, but it was not as obvious as the carbon fiber modified with polydopamine for 9 hours.
[0112] Test Example 3
[0113] Analysis of mechanical properties of carbon fiber / epoxy resin composites
[0114] 1. Interface shear strength test
[0115] V-notch shear performance test is one of the important means to macroscopically characterize the interface performance of composite materials. According to ASTMD5379 / D5379M-05 standard, the composite material is V-notched on the LE5105 microcomputer-controlled electronic composite material special testing machine (Shanghai Lishi Scientific Instrument Co., Ltd.), and the in-plane shear performance of the composite material is tested. The specific test size is as follows Fig.12 The loading speed is 1 mm / min, and three valid test data are taken for each sample. The in-plane shear strength is calculated according to formula (4):
[0116]
[0117] Where:
[0118] F u —ultimate strength, MPa;
[0119] Pu—lower value of the ultimate load and the load at which the shear strain is equal to 5%, N;
[0120] b—width of the composite material, mm;
[0121] d—thickness of composite material, mm.
[0122] The interface shear strength is mainly used to evaluate the strength and stability of the composite material in the shear direction, and can also be used to evaluate the bonding effect between the interfaces of the composite materials. Since the composite material sample did not suffer from fracture damage during the shear test, but torsion deformation, the maximum shear force within the shear strain of 5% was taken as the maximum shear force of the sample, and the shear strength of the sample was calculated according to formula (4). Fig.13The shear strength of the carbon fiber / epoxy resin composite material prepared by using the carbon fiber before and after modification as the reinforcement in Application Example 1, wherein CF, CF-C, 150W, 250W, 350W, and 450W respectively represent the composite materials prepared by using CF, CF-C, CF-C-PDA-150W (prepared in Example 2), CF-C-PDA (prepared in Example 1, sputtering power 250W), CF-C-PDA-350W (prepared in Example 3), and CF-C-PDA-450W (prepared in Example 4) as reinforcement. Fig.13 It can be seen that the interface shear strength of the composite material reinforced by surface-modified carbon fiber is higher than that of the composite material reinforced by unmodified carbon fiber. The interface shear strength of the composite material reinforced by CF-C modified by magnetron sputtering is 52.66MPa, which is 30.15% higher than that of the composite material reinforced by unmodified CF. The interface shear strength of the composite material reinforced by CF-C-PDA modified by magnetron sputtering and PDA is higher than that of the composite material reinforced by unmodified CF, with the maximum increase of 54.72% and the minimum increase of 38.7%; the interface shear strength of the composite material reinforced by CF-C modified by magnetron sputtering is increased by 18.88% and the minimum increase of 6.57%.
[0123] This is because the surface modification of single magnetron sputtering carbon fiber belongs to physical modification. After modification, the carbon fiber relies on the carbon particles deposited on its surface to enhance its roughness, thereby enhancing the bonding performance between the carbon fiber and the resin matrix. According to the previous analysis, the carbon fiber after magnetron sputtering / polydopamine composite modification not only changes the physical properties of the carbon fiber surface, but also increases the active groups, thereby improving the chemical bonding performance between the carbon fiber and the resin matrix, which can also be further explained by the shear stress-strain curve of the composite material.
[0124] Fig.14 This is the shear stress-strain curve of the carbon fiber / epoxy resin composite material prepared using the modified carbon fiber as reinforcement in Application Example 1. Normally, crack damage in a composite material first appears at the root of the notch in the specimen, and this is also the case in actual testing. When crack damage occurs in a composite material, it will cause a small load drop in the curve, which means that the first load drop in the stress-strain curve is the first crack damage in the composite material. Fig.14It can be seen that the time for the first crack damage of the composite material reinforced by CF-C-PDA after magnetron sputtering / PDA composite modification is delayed, and the required shear force is also increased. When the composite material reinforced by unmodified CF reaches the maximum in-plane shear stress, the in-plane shear stress of the composite material gradually decreases, while the composite material reinforced by CF-C modified by magnetron sputtering and the composite material reinforced by CF-C-PDA after magnetron sputtering and PDA composite modification show stress yield after reaching the maximum in-plane shear stress. When the shear strain is greater than 1.5%, the in-plane shear modulus of the composite material reinforced by CF-C-PDA after magnetron sputtering / PDA composite modification is significantly greater than the shear modulus of the composite material reinforced by CF and CF-C.
[0125] This is because when the composite material is subjected to in-plane shear load, the resin matrix at the notch is first cracked. Since the surface of the unmodified carbon fiber is smooth and the interface bonding performance with the resin matrix is poor, the load is directly transferred to the surface of the carbon fiber and extends along the interface, and then debonding failure occurs. Under the action of external force load, the carbon fiber is damaged. After the carbon fiber is modified by magnetron sputtering, the interface bonding performance between the carbon fiber and the resin matrix is enhanced due to the increase of surface cracks and surface roughness of the carbon fiber. When the resin matrix at the notch of the composite material is cracked, the in-plane shear load is transferred to the interface and the crack is deflected at the interface, which hinders the occurrence of cracks and changes the propagation of cracks, causing stress yielding of the carbon fiber composite material during in-plane shear. Under the action of continuous shear external force, the carbon fiber is damaged after debonding from the resin matrix. However, since the film layer deposited on the surface of the carbon fiber is formed by the accumulation of carbon particles, it has a certain degree of negative effect on the modulus of the carbon fiber composite material. The composite material with carbon fiber modified by magnetron sputtering / PAD as reinforcement has further improved the interfacial bonding performance between carbon fiber and resin matrix due to the increase of surface active functional groups and surface roughness. Therefore, under the action of in-plane shear load, the overall performance of carbon fiber epoxy resin-based composite material increases, delaying the time of crack appearance at the notch. At the same time, due to the adhesion property of polydopamine, it has a positive effect on the structural stability of the carbon film deposited on the carbon fiber surface, so the shear modulus of the carbon fiber composite material increases. As the in-plane shear load on the carbon fiber composite material continues to increase, the crack and load are transferred to the interface of the carbon fiber composite material, and the load and crack are deflected and extended at the interface. Therefore, the composite material also shows stress yield phenomenon under the action of in-plane shear load, delaying the shear damage of the composite material.
[0126] Bending performance test
[0127] In actual industrial applications, the flexural strength of composite materials is the test standard for evaluating the flexural properties of the entire material. In addition, the flexural strength is also determined to a certain extent by the interface bonding of the composite material. Although the bending normal stress is the main factor of material failure, under the action of load, the fiber composite material is also subject to internal shear failure, external surface pressure failure and fiber pressure failure. The composite material was subjected to a bending test in accordance with the three-point bending test in the ASTMD790 standard. The loading speed was 2mm / min and the span-to-thickness ratio was 32:1. The test data was for five valid specimens, and the flexural strength of the composite material was calculated according to formula (5):
[0128]
[0129] Where:
[0130] σ f —Flexural strength, MPa,
[0131] P—maximum load when the specimen is damaged, N;
[0132] L—span, mm;
[0133] B—specimen width, mm;
[0134] d—specimen thickness, mm.
[0135] Fig.15 The flexural strength of the carbon fiber / epoxy resin composite material prepared by using the carbon fiber before and after modification as the reinforcement in Application Example 1. Fig.15 As shown in the figure, the bending strength of the composite material with CF-C modified by magnetron sputtering as the reinforcement is 226.5MPa, which is 27.15% higher than that of the composite material with unmodified CF as the reinforcement, and the improvement effect is small. The bending strength of the composite material with CF-C-PDA modified by magnetron sputtering / PDA as the reinforcement is significantly improved. The bending strength of the composite material with CF-C-PDA (sputtering power is 250W) modified by magnetron sputtering / PDA as the reinforcement reaches 282.33MPa, which has the best improvement effect. The bending strength of the composite material with unmodified CF as the reinforcement is increased by 58.4%, and the bending strength of the composite metamaterial with CF-C modified by magnetron sputtering as the reinforcement is increased by 24.65%. The bending performance of the composite material is not only a reflection of the tensile and compressive combination performance, but also an enhancement of the interface performance of the composite material. Through analysis, it is shown that the interface performance of the composite material with carbon fiber modified by magnetron sputtering / PDA as the reinforcement is enhanced.
[0136] Fig.16 The bending stress-strain curves of the carbon fiber / epoxy resin composite material prepared by using the carbon fiber before and after modification as the reinforcement in Application Example 1 are shown in FIG. Fig.16 It can be seen that the bending rupture modulus of the composite material with surface-modified carbon fiber as reinforcement is larger than that of the composite material with unmodified carbon fiber as reinforcement. By comparison, it is also found that the bending modulus of the composite material with CF-C modified by magnetron sputtering as reinforcement is the largest. The composite material with unmodified CF as reinforcement did not show stress yield phenomenon during the bending fracture process, and the bending fracture was brittle fracture. The composite material with surface-modified carbon fiber as reinforcement showed obvious stress yield phenomenon. At the same time, it was also found that the bending fracture work of the composite material with carbon fiber reinforced by magnetron sputtering / PDA composite modification was increased, indicating that the bending toughness of the composite material with carbon fiber reinforced by magnetron sputtering / PDA composite modification was increased.
[0137] The reason for the above phenomenon is that magnetron sputtering deposits a carbon film on the surface of the carbon fiber, forming a transition interface between the modified carbon fiber and the resin matrix, which effectively slows down the transfer of stress load from the matrix to the fiber. After further modification by PDA, a polydopamine film is formed on the surface of the carbon fiber, and the interface bonding performance between the carbon fiber and the resin matrix is enhanced, further easing the transfer of stress between the interface layers, increasing the fracture work, and with the increase of magnetron sputtering power, the bending modulus of the composite material gradually decreases.
[0138] 3. Tensile performance test
[0139] The tensile properties of the composite materials were tested on a CSS-88100 universal testing machine (Changchun Mechanical Science Research Institute Co., Ltd.) according to ASTM D638. The tensile speed was set to 2 mm / min. Five valid data were tested for each sample. The tensile strength of the composite materials was calculated according to formula (6):
[0140]
[0141] Where: σ—tensile strength, MPa;
[0142] Pr—maximum load before failure, N;
[0143] b—width of the composite material, mm;
[0144] d—thickness of composite material, mm.
[0145] Fig.17For Application Example 1, the tensile strength of the carbon fiber / epoxy resin composite material prepared by using carbon fiber before and after modification as a reinforcement can be seen from the figure that the tensile strength of the composite material with CF-C modified by magnetron sputtering as a reinforcement reaches 102.39MPa, which is 11.01% higher than that of the composite material with unmodified CF as a reinforcement. The tensile strength of the composite material with carbon fiber modified by magnetron sputtering and PDA as a reinforcement is improved compared with the tensile strength of the composite material with unmodified carbon fiber as a reinforcement, but the increase of its tensile strength does not increase linearly with the increase of sputtering power, but increases first and then decreases with the increase of sputtering power. The tensile strength is the largest when the sputtering power is 250W, and the tensile strength reaches 201.94MPa, which is 1.1 times higher than that of the composite material with unmodified carbon fiber as a reinforcement, and 97.22% higher than that of the composite material with CF-C modified by magnetron sputtering as a reinforcement.
[0146] This is because microcracks are formed on the surface of the carbon fiber modified by magnetron sputtering, which plays a positive role in increasing the adhesion between the carbon fiber and the resin matrix. Active functional groups are introduced into the surface of the carbon fiber modified by magnetron sputtering / PDA, and the number of -OH and -NH on the surface of the carbon fiber increases, which is beneficial to the increase of the bonding performance between the carbon fiber and the resin matrix. After the bonding performance between the carbon fiber and the matrix resin is improved, when the resin matrix is subjected to external loads and cracks are generated, the stress can be effectively transferred through the interface to the carbon fiber, preventing the fiber from being pulled out and reducing damage to the interface.
[0147] Fig.18 The tensile stress-strain curves of the carbon fiber / epoxy resin composite material prepared by using the carbon fiber before and after modification as the reinforcement in Application Example 1 are shown in FIG. Fig.18 It can be found that the tensile damage of the composite material reinforced with unmodified carbon fiber is brittle fracture. The composite material directly breaks after reaching the maximum tensile modulus, and there is no stress yield phenomenon during the tensile fracture process. The composite material reinforced with carbon fiber modified by magnetron sputtering and PDA has obvious stress yield phenomenon during the tensile process. The tensile modulus partially increases, and does not increase linearly with the increase of sputtering power. The tensile modulus of the composite material reinforced with CF-C-PDA-250W increases the most, which obviously exceeds the tensile modulus of the composite material reinforced with unmodified carbon fiber; the tensile rupture modulus of the composite material reinforced with CF-C-PDA-350W is the smallest, which does not exceed the composite material reinforced with unmodified carbon fiber.
[0148] The main reason for the above situation is that carbon fiber is a brittle fiber. During the tensile fracture process, the carbon fiber and the resin matrix can be considered to be broken at the same time. However, after magnetron sputtering and PDA composite modification, a carbon film is formed on the surface of the carbon fiber, which has a strong transmission effect on the cracks formed during the tensile fracture of the composite material, which helps to delay the tensile fracture of the carbon fiber and enhance the tensile strength of the carbon fiber to a certain extent.
[0149] Fig.19 This is an optical microscope image of the tensile section of a carbon fiber / epoxy resin composite material prepared using carbon fibers before and after modification as reinforcement in Application Example 1, wherein CF(a), CF-C(b), 150W(c), 250W(d), 350W(e), and 450W(f) represent composite materials prepared using CF, CF-C, CF-C-PDA-150W (prepared in Example 2), CF-C-PDA (prepared in Example 1, sputtering power 250W), CF-C-PDA-350W (prepared in Example 3), and CF-C-PDA-450W (prepared in Example 4) as reinforcement, respectively. Fig.19 It can be seen that the tensile fracture section of the composite material reinforced by CF without surface modification is relatively neat (a), and the carbon fiber breaks simultaneously with the resin during the tensile fracture process. The tensile fracture of the composite material reinforced by CF-C modified by magnetron sputtering is also relatively neat (b). The tensile fracture of the composite material reinforced by carbon fiber modified by magnetron sputtering and PDA is jagged, and the fiber is pulled out at the fracture, and the resin is broken at the fracture (cf). During the tensile fracture process of the composite material, the carbon fiber and the resin matrix are not broken at the same time. The external resin matrix is subjected to force first, and the carbon fiber is then subjected to force through the interface transfer effect. During the tensile fracture process, the resin matrix and part of the fiber break first, and the fiber is pulled out. Then the remaining fiber bears all the tensile force, and the composite material finally breaks completely.
[0150] Fig. 20The cross-sectional SEM images of the carbon fiber / epoxy resin composite material prepared by using the carbon fiber before and after modification as the reinforcement in Application Example 1, wherein (a)-(c) represent the cross-sectional SEM images of the tensile specimens of the composite material with CF, CF-C, and CF-C-PDA as the reinforcement in Example 1, respectively, and (d)-(f) represent the longitudinal SEM images of the tensile specimens of the composite material with CF, CF-C, and CF-C-PDA as the reinforcement in Example 1 after fracture. From (a)-(c), it can be seen that the cross-sectional fibers of the composite material with unmodified CF as the reinforcement have more fiber extraction phenomena, and there are gaps between the carbon fiber and the resin. The fiber extraction of the composite material with CF-C modified by magnetron sputtering as the reinforcement is significantly improved, and the bonding between the fiber and the resin is improved to a certain extent. After the secondary modification of PDA, the fiber and the resin are tightly bonded at the fracture, and the number of holes, fiber exposure and fiber breakage is significantly improved. From the comparison of (d)-(f), it can be seen that there is more resin residue on the carbon fiber surface in the longitudinal plane of the composite material with modified carbon fiber as reinforcement, and the fiber surface in the fracture surface of the composite material with unmodified carbon fiber as reinforcement is smooth, with almost no residual resin. This shows that the modification strengthens the adhesion of epoxy resin to the carbon fiber surface, and the bonding performance between carbon fiber and resin is improved. This shows that the stress transfer at the interface layer between fiber and resin in the fracture process of the composite material with modified carbon fiber as reinforcement effectively hinders the fracture, indicating that the modification scheme is conducive to improving the mechanical properties of the composite material.
[0151] The embodiments described are only descriptions of the preferred modes of the present invention and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for modifying carbon fiber by constructing a "brick-mud" structure composite layer, characterized in that: The following steps are involved: The carbon fibers were sequentially subjected to surface modification treatments by magnetron sputtering and dopamine polymerization to form a carbon / polydopamine composite layer with a "brick-mud" structure on the surface of the carbon fibers.
2. The method according to claim 1, characterized in that The magnetron sputtering surface modification treatment is specifically to deposit a carbon film on the surface of the carbon fiber by magnetron sputtering.
3. The method according to claim 2, characterized in that The magnetron sputtering surface modification treatment uses carbon fiber as a substrate and carbon as a target material.
4. The method according to claim 3, characterized in that The sputtering conditions of the magnetron sputtering surface modification treatment include: a vacuum degree of 2×10 -3 Pa, the target-substrate distance is 4 cm, the sputtering power is 150-450 W, the sputtering pressure is 0.8-1.5 Pa, the sputtering time is 20-50 min, high-purity argon is used as the working gas, and the argon flow rate is 20 mL / min.
5. The method according to claim 1, characterized in that The dopamine polymerization surface modification treatment comprises: placing the carbon fiber subjected to the magnetron sputtering surface modification treatment into a dopamine solution and reacting for 6-12 hours.
6. The method according to claim 5, characterized in that The preparation method of the dopamine solution is as follows: after adjusting the pH value of the Tris buffer solution to 8.5, dopamine hydrochloride is added and stirred evenly to obtain the dopamine solution.
7. The method according to claim 6, characterized in that The concentration of the Tris buffer solution is 0.01 mol / L; the amount of dopamine hydrochloride added is 2 g / L.
8. A composite modified carbon fiber prepared by modifying carbon fiber according to the method described in any one of claims 1 to 7.
9. Use of the composite modified carbon fiber as claimed in claim 8 as a reinforcement in preparing a composite material.
10. A carbon fiber / epoxy resin composite material, characterized in that: The composite modified carbon fiber as claimed in claim 8 is used as a reinforcement, and the epoxy resin and a curing agent are used as a matrix.
Citation Information
Cited By
Preparation method of Mg (OH) 2 / polydopamine multi-scale synergistic modified carbon fiber / epoxy resin composite material
CN119684742A
Laser synergistic modified polydopamine metallized carbon fiber material and preparation method thereof
CN121802683A