Environment-friendly degradable polyurethane composite leather and preparation method thereof

By using polylactic acid-based polyurethane, PBAT polyurethane and water-based polyurethane in the preparation of polyurethane composite leather, the problem of high solvent use and production costs in the prior art is solved, and environmentally friendly, degradable and high-performance polyurethane composite leather is realized , meet the needs of passenger cars.

CN118932736AInactive Publication Date: 2024-11-12SEIREN SUZHOU CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411190597.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing polyurethane synthetic leather uses a large number of harmful solvents during the preparation process, and the production cost of water-based polyurethane synthetic leather is high and its physical properties are degraded, making it difficult to meet environmental protection and performance requirements.

Method used

Using the preparation method of environmentally friendly and degradable polyurethane composite leather, the specific components and processes of the surface layer, followed by the surface treatment layer, including polylactic acid-based polyurethane, PBAT polyurethane and water-based polyurethane, avoid the use of a large number of harmful solvents, and improve the use of The strength and wear resistance of composite leather.

Benefits of technology

It has achieved low-carbon, low-energy consumption, zero-emission environmentally friendly and degradable composite leather, with excellent degradability, photo-resistant aging effect and high environmental protection, and meets the physical and chemical performance requirements of passenger cars.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932736A_ABST
    Figure CN118932736A_ABST
Patent Text Reader

Abstract

The invention discloses environment-friendly degradable polyurethane composite leather and a preparation method thereof.The preparation method comprises the following steps that S1, a surface layer solution is prepared firstly, then defoaming treatment is carried out, coating processing is carried out on release paper, and drying forming is carried out; s2, firstly preparing a bonding layer solution, then carrying out coating processing on the surface layer, and carrying out drying forming; s3, the bonding layer and the non-woven fabric layer of the product obtained in the S2 are bonded together, and a composite leather blank is formed; s4, stripping the composite leather blank from the release paper to obtain the composite leather blank; s5, curing the composite leather blank obtained in the step S4, and cooling; and S6, preparing a surface treatment layer solution, coating the surface layer of the composite leather blank obtained in the step S5 with the surface treatment layer solution, and then baking and forming to obtain the finished product composite leather. The strength of the composite leather can be improved, the leather is biodegradable, the product competitiveness is improved, and a large number of harmful solvents do not need to be added in the preparation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane composite materials, and in particular to an environmentally friendly and degradable polyurethane composite leather and a preparation method thereof. Background Art

[0002] In the field of materials, the application of biodegradable bio-based materials in the field of passenger cars has always been the direction of the automotive industry. Among them, biodegradable polyurethane products, environmentally friendly solvent-free synthetic leather, are suitable for interior decoration and will be the dominant direction of interior decoration materials for passenger cars in the future.

[0003] At present, polyurethane synthetic leather on the market can be mainly divided into two categories: solvent-based polyurethane synthetic leather, water-based polyurethane synthetic leather and solvent-free polyurethane synthetic leather. Among them, solvent-based polyurethane synthetic leather has the largest market share. This product has excellent performance and low cost, but solvent-based polyurethane synthetic leather needs to add a large amount of harmful dimethylformamide (DMF) solvent during the preparation process, and the solvent is difficult to completely recover; although water-based polyurethane synthetic leather uses water instead of organic solvent as a dispersion medium, it can avoid the introduction of a large amount of harmful organic solvents, but the removal of the water medium in the later stage requires a lot of energy, which leads to a significant increase in production costs, and the physical properties of the synthetic leather will also be reduced.

[0004] In order to solve the above problems in the prior art, the present invention is provided. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide an environmentally friendly and degradable polyurethane composite leather and a preparation method thereof.

[0006] The technical solution of the present invention is:

[0007] The present invention relates to a method for preparing an environmentally friendly and degradable polyurethane composite leather, comprising the following steps:

[0008] S1 Surface layer preparation: first prepare the surface layer solution, then degassing, coating on release paper, and then drying and forming;

[0009] S2 Adhesive layer preparation: first prepare the adhesive layer solution, then coat it on the surface layer, and then dry it to form;

[0010] S3 bonding and laminating: bonding and laminating the adhesive layer and the non-woven fabric layer of the product obtained in step S2 together to form a composite leather blank;

[0011] S4 peeling: peeling the composite leather blank obtained in step S3 from the release paper to obtain the composite leather blank;

[0012] S5 aging treatment: aging the composite leather blank obtained in step S4 in an oven and cooling;

[0013] S6 Surface layer treatment: preparing a surface treatment layer solution, coating the surface treatment layer solution on the surface layer of the composite leather blank obtained in S5, and then baking and forming to obtain a finished composite leather.

[0014] Preferably, the surface layer solution includes polylactic acid-based polyurethane, a bridging agent, a pigment and a dissolving medium, and the amount of each material is as follows by weight: 60.0 to 70.0 parts of polylactic acid-based polyurethane, 2.0 to 4.0 parts of a bridging agent, 10.0 to 15.0 parts of a pigment, and 15.0 to 20.0 parts of a dissolving medium. The specific composition of the pigment varies according to the color of the product.

[0015] Preferably, the bonding layer solution includes polyurethane, a hardener, a catalyst and a flame retardant, and the amount of each material is as follows by weight: 26.0-30.0 parts of polyurethane, 45.0-50.0 parts of hardener, 1.0-3.0 parts of catalyst, and 18.0-25.0 parts of flame retardant. More preferably, the polyurethane is PBAT (polybutylene terephthalate), the hardener is an aliphatic diisocyanate, the catalyst is an amine organic acid salt, and the flame retardant is a phosphorus flame retardant.

[0016] Preferably, the surface treatment layer solution includes water-based polyurethane, a bridging agent, a thickener and a smoothing agent. The amount of each material used, in parts by mass, is as follows: 85.0 to 95.0 parts of water-based polyurethane, 2.0 to 4.0 parts of a bridging agent, 1.0 to 3.0 parts of a thickener, and 3.0 to 7.0 parts of a smoothing agent; further preferably, the bridging agent is carbodiimide, the thickener is an alkaline thickener, such as an acrylic polymer, and the smoothing agent is a silicon-based agent and its silicon polymer.

[0017] Preferably, in step S1, the stirring speed of preparing the surface layer solution is 350 rpm to 450 rpm, the stirring time is 30 min to 60 min, and the viscosity of the obtained surface layer solution is 3000 cps to 5500 cps;

[0018] The treatment time of the surface layer solution degassing treatment is 40min to 60min; the prepared surface layer solution is degassed by a circulating degassing machine to fully ensure the degassing effect, so that when the surface layer solution is circulated and used, air is prevented from entering during the transportation process, so as to improve the surface layer coating quality;

[0019] The surface layer solution coating processing speed is 9.0m / min~11.0m / min, and the usage is 80g / m 2 ~120g / m 2 ;

[0020] The surface layer drying and molding temperature is 100℃~130℃, the oven length is 30m, and the baking time is 2.7min~3.3min.

[0021] Preferably, in step S2, the stirring speed of preparing the bonding layer solution is 2300 rpm to 2500 rpm, and the stirring time is 48-60 hours;

[0022] The coating speed of the adhesive layer solution is 9.0m / min~11.0m / min, and the usage is (225±25)g / m 2 ;

[0023] The drying and molding temperature of the next layer is 90°C to 110°C, the length of the oven is 30m, the baking time is 2.7min to 3.3min; the drying degree of the next layer is 80% to 90%.

[0024] Preferably, in step S6, the stirring speed of the surface treatment layer solution is 350 rpm to 450 rpm, the stirring time is 30 min to 60 min, and the viscosity of the surface treatment layer solution is 500 cps to 700 cps;

[0025] The surface treatment layer liquid coating speed is 9.0m / min~11.0m / min, and the amount used is 40g / m 2 ~50g / m 2 ;

[0026] The baking temperature of the surface treatment layer is 100°C to 130°C, the length of the oven is 28m, and the baking time is 2.5min to 3.1min.

[0027] Preferably, the thickness of the nonwoven fabric layer is (800±100) μm, and its mass surface density is (225±25) g / m 2 , and modified PLA nonwoven fabric is further preferred.

[0028] Preferably, the production environment temperature of steps S1 to S6 is 0.0° C. to 35.0° C., and the production environment humidity is 25% to 75%.

[0029] Preferably, in step S3, the bonding speed is 9.0 m / min to 11.0 m / min, and the bonding pressure is 0.25 MPa to 0.35 MPa.

[0030] Preferably, in step S5, the aging treatment temperature is 125° C. to 135° C., the oven length is 120 m, and the baking time is 10.9 min to 13.3 min.

[0031] The present invention also relates to an environmentally friendly and degradable polyurethane composite leather, which is prepared by the above-mentioned preparation method and includes a composite leather blank and a surface treatment layer. The composite leather blank includes a non-woven fabric layer, a bonding layer and a surface layer arranged in sequence, and the surface treatment layer is arranged on the surface layer.

[0032] The beneficial effects of the present invention are:

[0033] 1. The environmentally friendly and degradable polyurethane composite leather of the present invention improves the strength of the composite leather through the specific components of polylactic acid-based polyurethane raw materials and composite leather structure, as well as the component performance and preparation process of the product, thereby achieving the purpose of improving the product life and improving the product competitiveness. It is biodegradable, harmless to the human body during use, does not pollute the environment, and the degradation products will not cause new pollution to the environment, thereby achieving low carbon, low energy consumption, zero emissions or low emissions.

[0034] 2. The environmentally friendly and degradable composite leather of the present invention includes a non-woven fabric layer, an adhesive layer, a surface layer and a surface treatment layer. By improving the raw materials of the surface layer and the adhesive layer and applying new materials, the surface layer can enhance the surface film-forming and wear resistance, improve the flexibility of the product, and form a stable film strength. The composite leather not only has excellent degradable properties, higher environmental protection and sustainability, but also has excellent light aging resistance, and can effectively meet the physical and chemical properties of passenger cars.

[0035] 3. In the preparation of composite leather, the materials of the surface layer, the adhesive layer and the surface treatment layer are all different, wherein the surface layer uses polylactic acid-based polyurethane, the adhesive layer uses PBAT polyurethane, and the surface treatment layer uses water-based polyurethane. There is no need to add a large amount of harmful dimethylformamide solvent, and only water as a dissolving medium is used in the preparation of the surface layer solution, and the amount used is relatively small. Even if the amount of water used is further reduced, the performance of the composite leather will not be significantly reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:

[0037] Figure 1 This is a process flow chart of a method for preparing an environmentally friendly and degradable polyurethane composite leather according to the present invention;

[0038] Figure 2 It is a schematic diagram of the cross-sectional structure of an environmentally friendly and degradable polyurethane composite leather of the present invention;

[0039] Figure 3 It is a graph showing the degradation rate of degradable materials.

[0040] Markings in the figure: 1- non-woven fabric layer, 2- adhesive layer, 3- surface layer, 4- surface treatment layer. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0042] The invention provides an environmentally friendly and degradable polyurethane composite leather, which comprises a non-woven fabric layer, a bonding layer, a surface layer and a surface treatment layer which are arranged in sequence.

[0043] First, prepare the release paper and non-woven fabric layer. The non-woven fabric layers used in the following examples and comparative examples are all modified PLA non-woven fabrics with a thickness of (800±100) μm and a mass surface density of (225±25) g / m 2 The production environment temperature is 0.0℃~35.0℃, and the production environment humidity is 25%~75%.

[0044] The raw materials used in the following examples and comparative examples are:

[0045] Polylactic acid-based polyurethane (water-based, solid content 39%-51%);

[0046] Amine organic acid salt catalyst (solvent-free polyurethane C component);

[0047] Phosphorus flame retardant (organic phosphate aliphatic phosphoric acid amide, powdery white body, particle size D50);

[0048] Water-based polyurethane used for the surface treatment layer (water-based, solid content 40%-60%);

[0049] Thickener Ⅰ, polyacrylic acid emulsion (solid content 5%-10%);

[0050] Thickener II (solid content 25%-30%);

[0051] Smoothing agent (solid content 100%).

[0052] Example 1

[0053] S1 surface layer production:

[0054] (1) According to the material components of the surface layer, raw materials are prepared according to the following weight parts: 60.0 parts of polylactic acid-based polyurethane, 2.0 parts of bridging agent carbodiimide, 10.0 parts of inorganic pigments iron oxide and carbon black (the weight ratio of iron oxide to carbon black is 2:4), and 18.0 parts of dissolving medium water;

[0055] (2) Mixing the raw materials prepared in step (1) to prepare a surface layer solution, the stirring speed of the surface layer solution is 350 rpm, the stirring time is 30 min, and the viscosity of the surface layer solution is 3000 cps;

[0056] (3) The surface layer solution is fully degassed for 40 min;

[0057] (4) The surface layer solution is coated on the release paper at a coating speed of 9 m / min and a usage of 80 g / m 2 ;

[0058] (5) Then the mold is dried at a temperature of 100°C, an oven length of 30 m, and a drying time of 3.3 min.

[0059] S2 next layer production:

[0060] (1) According to the material components of the adhesive layer, the raw materials are prepared according to the following mass parts: 26.0 parts of PBAT polyurethane, 45.0 parts of hexamethylene diisocyanate HDI, 1.0 parts of amine catalyst, and 18.0 parts of phosphorus flame retardant;

[0061] (2) Mixing the raw materials prepared in step (1) to prepare a bonding layer solution, wherein the bonding layer solution is stirred at a speed of 2300 rpm for 60 h;

[0062] (3) The bonding layer solution was coated on the surface layer at a coating speed of 9.0 m / min and a usage of 200 g / m 2 ;

[0063] (4) Then, the adhesive layer is dried and formed. The drying and forming temperature of the adhesive layer is 90° C., the length of the oven is 30 m, the baking time is 3.3 min, and the drying degree of the adhesive layer is 80%.

[0064] S3 bonding and laminating: bonding the adhesive layer and the non-woven fabric layer of the product obtained in step S2 together to form a composite leather blank; the bonding speed is 9.0 m / min, and the bonding pressure is 0.25 MPa.

[0065] S4 peeling: peeling the composite leather blank obtained in step S3 from the release paper to obtain the composite leather blank.

[0066] S5 aging treatment: the composite leather blank in step S4 is aged in an oven and then cooled to obtain an aged leather blank; the aging treatment temperature is 125° C., the oven length is 120 m, and the baking time is 13.3 min.

[0067] S6 surface treatment:

[0068] (1) According to the material components of the surface treatment layer liquid of the surface treatment layer, the raw materials are prepared according to the following weight parts: 85.0 parts of water-based polyurethane, 2.0 parts of bridging agent carbodiimide, 1.0 parts of thickener I polyacrylic acid emulsion, and 3.0 parts of smoothing agent silicon;

[0069] (2) Mixing the raw materials prepared in step (1) to prepare a surface treatment layer liquid, wherein the stirring speed of the surface treatment layer liquid is 350 rpm, the stirring time is 30 min, and the viscosity of the surface treatment layer liquid is 500 cps;

[0070] (3) The surface treatment layer liquid is coated on the surface layer of the matured leather blank obtained in S4, and the coating speed is 9.0 m / min and the usage amount is 40 g / m 2 , and then baked and formed, the baking and forming temperature is 100℃, the oven length is 28m, and the baking time is 3.1min.

[0071] The environmentally friendly and biodegradable polyurethane composite leather prepared according to the above method was tested for performance. The results are shown in Table 1.

[0072] Example 2

[0073] This embodiment provides another environmentally friendly and degradable polyurethane composite leather and a preparation method thereof, which differs from Embodiment 1 in that steps S1, S2 and S6 are:

[0074] S1 surface layer production:

[0075] (1) According to the material components of the surface layer, raw materials are prepared according to the following weight parts: 70.0 parts of polylactic acid-based polyurethane, 4.0 parts of bridging agent carbodiimide, 15.0 parts of inorganic pigments iron oxide and carbon black (the weight ratio of iron oxide to carbon black is 2:4), and 20.0 parts of dissolving medium water;

[0076] (2) mixing the raw materials prepared in step (1) to prepare a surface layer solution, wherein the stirring speed of the surface layer solution is 450 rpm, the stirring time is 60 min, and the viscosity of the surface layer solution is 5000 cps;

[0077] (3) The surface layer solution is fully degassed for 60 min;

[0078] (4) The surface layer solution is coated on the release paper at a coating speed of 11 m / min and a usage of 120 g / m 2 ;

[0079] (5) Then the surface layer is dried and formed at a temperature of 130°C, an oven length of 30 m, and a baking time of 2.7 min.

[0080] S2 next layer production:

[0081] (1) According to the material components of the adhesive layer, the raw materials are prepared according to the following weight parts: 30.0 parts of PBAT polyurethane, 50.0 parts of hexamethylene diisocyanate HDI, 3.0 parts of amine organic acid salt catalyst, and 25.0 parts of phosphorus flame retardant;

[0082] (2) Mixing the raw materials prepared in step (1) to prepare a bonding layer solution, wherein the bonding layer solution is stirred at a speed of 2500 rpm for 48 hours;

[0083] (3) The bonding layer solution was coated on the surface layer at a coating speed of 11 m / min and a usage of 250 g / m 2 ;

[0084] (4) Then, the film is dried and formed. The drying and forming temperature is 110° C., the oven length is 30 m, the baking time is 2.7 min, and the drying degree of the bonding layer is 90%.

[0085] S6 surface treatment:

[0086] (1) According to the material components of the surface treatment layer liquid of the surface treatment layer 4, the raw materials are prepared according to the following weight parts: 95.0 parts of waterborne polyurethane, 4.0 parts of bridging agent carbodiimide, 3.0 parts of thickener I polyacrylic acid emulsion, and 7.0 parts of smoothing agent silicon;

[0087] (2) Mixing the raw materials prepared in step (1) to prepare a surface treatment layer liquid, wherein the stirring speed of the surface treatment layer liquid is 450 rpm, the stirring time is 60 min, and the viscosity of the surface treatment layer liquid is 700 cps;

[0088] (3) The surface treatment layer liquid is coated on the surface layer of the matured leather blank obtained in S4, and the coating speed is 11.0 m / min and the usage amount is 50 g / m 2 ;

[0089] (4) Then the mold is dried and formed. The baking temperature is 130°C, the oven length is 28m, and the baking time is 2.5min.

[0090] The environmentally friendly and biodegradable polyurethane composite leather prepared according to the above method was tested for performance. The results are shown in Table 1.

[0091] Embodiment 3:

[0092] This embodiment provides another environmentally friendly and degradable polyurethane composite leather and a preparation method thereof, which differs from the embodiment 1 in that steps S1, S2 and S6 are:

[0093] S1 surface layer production:

[0094] (1) According to the material components of the surface layer, raw materials were prepared according to the following weight parts: 65.0 parts of polylactic acid-based polyurethane, 3.0 parts of bridging agent carbodiimide, 13 parts of inorganic pigments iron oxide and carbon black (the weight ratio of iron oxide to carbon black was 2:4), and 19.0 parts of dissolving medium water;

[0095] (2) Mixing the raw materials prepared in step (1) to prepare a surface layer solution, wherein the stirring speed of the surface layer solution is 400 rpm, the stirring time is 45 min, and the viscosity of the surface layer solution is 4500 cps;

[0096] (3) The surface layer solution is fully degassed for 50 min;

[0097] (4) The surface layer solution is coated on the release paper at a coating speed of 10.0 m / min and a usage of 100 g / m 2 ;

[0098] (5) Then the surface layer is dried and formed at a temperature of 115°C, an oven length of 30 m, and a drying time of 3.0 min.

[0099] S2 next layer production:

[0100] (1) According to the material components of the adhesive layer, the raw materials are prepared according to the following weight parts: 28.0 parts of PBAT polyurethane, 48.0 parts of hexamethylene diisocyanate HDI, 2.0 parts of amine organic acid salt catalyst, and 22.0 parts of phosphorus flame retardant;

[0101] (2) Mixing the raw materials prepared in step (1) to prepare a bonding layer solution, the bonding layer solution was stirred at a speed of 2400 rpm for 54 h;

[0102] (3) The bonding layer solution was coated on the surface layer at a coating speed of 10.0 m / min and a usage of 225 g / m 2 ;

[0103] (4) Then the product is dried and formed at a temperature of 100° C. for 3 minutes, and the drying degree of the next layer is 85%.

[0104] S6 surface treatment:

[0105] (1) According to the material components of the surface treatment layer liquid of the surface treatment layer, the raw materials are prepared according to the following weight parts: 90.0 parts of water-based polyurethane, 3.0 parts of bridging agent carbodiimide, 2.0 parts of thickener II, and 5.0 parts of smoothing agent silicon;

[0106] (2) Mixing the raw materials prepared in step (1) to prepare a surface treatment layer liquid, wherein the stirring speed of the surface treatment layer liquid is 450 rpm, the stirring time is 45 min, and the viscosity of the surface treatment layer liquid is 600 cps;

[0107] (3) The surface treatment layer liquid is coated on the surface layer of the matured leather blank obtained in S4, and the coating speed is 10.0 m / min and the usage amount is 45 g / m 2 ;

[0108] (4) Then the mold is dried and formed. The baking temperature is 120°C, the oven length is 28m, and the baking time is 2.8min.

[0109] Comparative Example 1

[0110] This comparative example provides an environmentally friendly and degradable polyurethane composite leather and a preparation method thereof, which differs from Example 3 in steps S1 and S2:

[0111] S1 surface layer production:

[0112] (1) According to the material components of the surface layer, raw materials were prepared according to the following weight parts: 65.0 parts of polylactic acid-based polyurethane, 3.0 parts of bridging agent carbodiimide, 13 parts of inorganic pigments iron oxide and carbon black (the weight ratio of iron oxide to carbon black was 2:4), and 16.0 parts of dissolving medium water;

[0113] (2) Mixing the raw materials prepared in step (1) to prepare a surface layer solution, the stirring speed of the surface layer solution is 400 rpm, the stirring time is 45 min, and the viscosity of the surface layer solution is 5300 cps;

[0114] (3) The surface layer solution is fully degassed for 50 min;

[0115] (4) The surface layer solution is coated on the release paper at a coating speed of 10.0 m / min and a usage of 100 g / m 2 ;

[0116] (5) Then the surface layer is dried and formed at a temperature of 115°C, an oven length of 30 m, and a drying time of 3.0 min.

[0117] S2 next layer production:

[0118] (1) According to the material components of the adhesive layer, the raw materials are prepared according to the following weight parts: 28.0 parts of PBAT polyurethane, 48.0 parts of hexamethylene diisocyanate HDI, 2.0 parts of amine organic acid salt catalyst, and 22.0 parts of phosphorus flame retardant;

[0119] (2) Mixing the raw materials prepared in step (1) to prepare a bonding layer solution, the bonding layer solution was stirred at a speed of 2400 rpm for 51 h;

[0120] (3) The bonding layer solution was coated on the surface layer at a coating speed of 10.0 m / min and a usage of 225 g / m 2 ;

[0121] (4) Then the product is dried and formed at a temperature of 100° C. for 3 minutes, and the drying degree of the next layer is 85%.

[0122] Comparative Example 2

[0123] This comparative example provides an environmentally friendly and degradable polyurethane composite leather and a preparation method thereof, which is different from comparative example 1 in that step S1:

[0124] S1 surface layer production:

[0125] (1) According to the material components of the surface layer, raw materials were prepared according to the following weight parts: 65.0 parts of polylactic acid-based polyurethane, 3.0 parts of bridging agent carbodiimide, 13 parts of inorganic pigments iron oxide and carbon black (the weight ratio of iron oxide to carbon black was 2:4), and 15.0 parts of dissolving medium water;

[0126] (2) Mixing the raw materials prepared in step (1) to prepare a surface layer solution, the stirring speed of the surface layer solution is 400 rpm, the stirring time is 45 min, and the viscosity of the surface layer solution is 5500 cps;

[0127] (3) The surface layer solution is fully degassed for 50 min;

[0128] (4) The surface layer solution is coated on the release paper at a coating speed of 10.0 m / min and a usage of 100 g / m 2 ;

[0129] (5) Then the surface layer is dried and formed at a temperature of 115°C, an oven length of 30 m, and a drying time of 3.0 min.

[0130] The environmentally friendly and biodegradable polyurethane composite leather prepared according to the above method was tested for performance. The results are shown in Table 1.

[0131] Table 1 Performance test table of water-friendly biodegradable polyurethane composite leather

[0132]

[0133] Through the above embodiments, we can know that the performance of the environmentally friendly and degradable polyurethane composite leather of the present invention is improved. Under different deformation conditions, the strength of the environmentally friendly and degradable polyurethane composite leather fluctuates slightly, but does not affect the overall leather performance. It fully meets the quality requirements of passenger cars and has broad application prospects.

[0134] In addition, the degradation mechanism was also studied to degrade polymer materials more effectively. The main degradation mechanisms include biological, light, thermal and solvent degradation. The table shows the degradation rate changes of degradable materials at different time points; this transition table is compiled from laboratory transition results, and the actual degradation rate will depend on the type of material, degradation conditions (such as temperature, humidity, microbial activity and solvent degradation, etc.) and test methods. In addition, the degradation rates of different materials under different conditions may vary greatly.

[0135] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.

Claims

1. A method for preparing an environmentally friendly and degradable polyurethane composite leather, comprising the following steps: S1 Surface layer preparation: first prepare the surface layer solution, then degassing, coating on release paper, and then drying and forming; S2 Adhesive layer preparation: first prepare the adhesive layer solution, then coat it on the surface layer, and then dry it to form; S3 bonding and laminating: bonding and laminating the adhesive layer and the non-woven fabric layer of the product obtained in step S2 together to form a composite leather blank; S4 peeling: peeling the composite leather blank obtained in step S3 from the release paper to obtain the composite leather blank; S5 aging treatment: aging the composite leather blank obtained in step S4 in an oven and cooling; S6 Surface layer treatment: preparing a surface treatment layer solution, coating the surface treatment layer solution on the surface layer of the composite leather blank obtained in S5, and then baking and forming to obtain a finished composite leather.

2. The preparation method according to claim 1, characterized in that: The surface layer solution includes polylactic acid-based polyurethane, a bridging agent, a pigment and a dissolving medium. The amount of each material is as follows, calculated by weight: 60.0 to 70.0 parts of polylactic acid-based polyurethane, 2.0 to 4.0 parts of a bridging agent, 10.0 to 15.0 parts of a pigment, and 15.0 to 20.0 parts of a dissolving medium.

3. The preparation method according to claim 1, characterized in that: The bonding layer solution includes polyurethane, a hardener, a catalyst and a flame retardant. The amount of each material is as follows, calculated by weight: 26.0 to 30.0 parts of polyurethane, 45.0 to 50.0 parts of hardener, 1.0 to 3.0 parts of catalyst, and 18.0 to 25.0 parts of flame retardant.

4. The preparation method according to claim 1, characterized in that: The surface treatment layer solution includes water-based polyurethane, a bridging agent, a thickener and a smoothing agent. The amount of each material used is as follows, calculated by weight: 85.0 to 95.0 parts of water-based polyurethane, 2.0 to 4.0 parts of a bridging agent, 1.0 to 3.0 parts of a thickener, and 3.0 to 7.0 parts of a smoothing agent.

5. The preparation method according to claim 1, characterized in that: In step S1, the stirring speed of the surface layer solution is 350 rpm to 450 rpm, the stirring time is 30 min to 60 min, and the viscosity of the surface layer solution is 3000 cps to 5500 cps; The treatment time of degassing treatment of the surface layer solution is 40min to 60min; The surface layer solution coating processing speed is 9.0m / min~11.0m / min, and the usage is 80g / m 2 ~120g / m 2 ; The surface layer drying and molding temperature is 100°C to 130°C, and the baking time is 2.7min to 3.3min.

6. The preparation method according to claim 1, characterized in that: In step S2, the stirring speed of preparing the bonding layer solution is 2300 rpm to 2500 rpm, and the stirring time is 48-60 hours; The coating speed of the adhesive layer solution is 9.0m / min~11.0m / min, and the usage is (225±25)g / m 2 ; The drying and molding temperature of the next layer is 90° C. to 110° C., and the baking time is 2.7 min to 3.3 min. The drying degree of the next layer is 80% to 90%.

7. The preparation method according to claim 1, characterized in that: In step S6, the stirring speed of the surface treatment layer solution is 350 rpm to 450 rpm, the stirring time is 30 min to 60 min, and the viscosity of the surface treatment layer solution is 500 cps to 700 cps; The surface treatment layer liquid coating speed is 9.0m / min~11.0m / min, and the amount used is 40g / m 2 ~50g / m 2 ; The baking temperature of the surface treatment layer is 100°C to 130°C, and the baking time is 2.5min to 3.1min.

8. The preparation method according to claim 1, characterized in that: The thickness of the nonwoven layer is (800±100)μm, and its mass surface density is (225±25)g / m 2 .

9. The preparation method according to any one of claims 1 to 8, characterized in that: The production environment temperature of step S1 to step S6 is 0.0°C to 35.0°C, and the production environment humidity is 25% to 75%.

10. An environmentally friendly and degradable polyurethane composite leather, characterized in that: The leather product is prepared by the preparation method according to any one of claims 1 to 9, comprising a composite leather stock and a surface treatment layer, wherein the composite leather stock comprises a non-woven fabric layer, a bonding layer and a surface layer arranged in sequence, and the surface treatment layer is arranged on the surface layer.

Citation Information

Patent Citations

  • Method for preparing aqueous polyurethane adhesive and superfine fiber synthetic leather

    CN101665675A

  • Biological leather and manufacturing method thereof

    CN113481734A

  • PU (Polyurethane) composite leather and preparation method thereof

    CN113605107A

  • Solvent-free polylactic acid bio-based polyurethane synthetic leather, preparation method and application

    CN113699802A

  • Biodegradable TPU synthetic leather and preparation method thereof

    CN115162013A