Natural dye dyed polyurethane microfiber leather and preparation method thereof

Natural dye-dyed polyurethane microfiber leather is prepared by chemically reacting dyes extracted from natural plants with polyurethane resin. This method solves the problems of low color fastness and environmental pollution caused by chemically synthesized dyes, achieving high color fastness and environmentally friendly dyeing effects, and endowing synthetic leather with multiple functions.

CN118932738APending Publication Date: 2024-11-12ZHEJIANG MEISHENG NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411322014.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When existing chemically synthesized dyes are used for dyeing microfiber leather, there are problems such as low color fastness and easy environmental pollution.

Method used

Natural dye-dyed polyurethane microfiber leather is prepared by chemically reacting dyes extracted from natural plants with polyurethane resin to form covalent bonds. The process includes the extraction of plant dyes, rotary evaporation, freeze drying, mixing reaction and coating process.

Benefits of technology

The prepared natural dye-dyed polyurethane microfiber leather has high color fastness, is environmentally friendly and pollution-free, and endows synthetic leather with antibacterial, antioxidant and UV protection functions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005054257400000111
    Figure BDA0005054257400000111
Patent Text Reader

Abstract

The invention belongs to the technical field of polyurethane microfiber leather dyeing, and provides natural dye dyed polyurethane microfiber leather and a preparation method thereof. The preparation method mainly comprises the following steps: extracting the vegetable dye, preparing the colored polyurethane emulsion and preparing the polyurethane microfiber leather dyed by the natural dye. The preparation method provided by the invention is relatively simple in process and relatively low in cost, saves energy, avoids participation of chemical dyes, and has the advantages of being green, environment-friendly, free of environmental pollution and the like. And the polyurethane microfiber leather dyed by the natural dye prepared by the invention is relatively complete in color system, bright in color and high in color fastness, and also has antibacterial and ultraviolet-proof functions and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane microfiber leather dyeing, in particular to polyurethane microfiber leather dyed with natural dyes and a preparation method thereof. Background Art

[0002] Natural leather is rich in collagen and has good moisture permeability, air permeability and wear resistance due to its unique three-dimensional woven structure, which is very popular among people. At present, the raw materials for the production of natural leather are mainly animal fur. As human awareness of animal protection gradually increases, the use of synthetic leather to replace natural leather has attracted more and more attention. Synthetic leather has replaced natural leather with insufficient resources. It is widely used in luggage, clothing, sofas, car interiors, shoes and other fields, and has broad development prospects. However, with the improvement of people's living standards and aesthetic needs, consumers have higher and higher requirements for the appearance, physical properties and feel of leather.

[0003] Superfine synthetic leather can be comparable to natural leather in terms of appearance texture, physical properties and wearing comfort, but it still has a certain gap with natural leather in dyeing. In addition, due to the different structures of the superfine fibers and polyurethane resins in the superfine leather, there are differences in the dyeing performance of the dye to the superfine fibers and water-based polyurethane, which makes the superfine leather have problems such as low dyeing rate, dye penetration, level dyeing and friction color fastness during dyeing. Therefore, improving the dyeing rate and color fastness of colored superfine leather has become a necessary trend of development. At present, acid dyes, metal complex dyes, neutral dyes, disperse dyes or pigments are mostly used to color synthetic leather, and the use of these chemical synthetic dyes increases the chromaticity of wastewater, which easily causes water pollution. Therefore, how to provide a more natural and environmentally friendly dye to dye superfine synthetic leather has become a problem that those skilled in the art need to solve urgently. Summary of the invention

[0004] In view of this, the present invention provides a natural dye-dyed polyurethane microfiber leather and a preparation method thereof, the purpose of which is to solve the technical problems of existing chemical synthetic dyes such as low color fastness and easy environmental pollution.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The invention provides a method for preparing polyurethane microfiber leather dyed with natural dyes, comprising the following steps:

[0007] S1, immersing natural plants in water for extraction to obtain a plant dye extract, and performing rotary evaporation and freeze drying on the plant dye extract to obtain a plant dye;

[0008] S2, mixing the plant dye, diol, diisocyanate and catalyst and reacting them to obtain an intermediate;

[0009] S3, mixing the intermediate and the chain extender and reacting them to obtain a prepolymer;

[0010] S4, mixing the prepolymer, polyamine, water and ethylenediamine and reacting them to obtain a colored waterborne polyurethane emulsion;

[0011] S5, coating the aqueous polyurethane emulsion on the substrate and pre-baking to form a coating, hot-pressing the coating and the base fabric, and then aging, cooling, peeling, and winding in sequence to obtain natural dye-dyed polyurethane microfiber leather.

[0012] Furthermore, in step S1, the mass volume ratio of natural plants and water is 1 g: 50-100 mL; the extraction temperature is 30-80° C., and the extraction time is 30-60 min.

[0013] Furthermore, in step S2, the mass ratio of diol to diisocyanate is 3-7:3-7, the amount of plant dye used is 5-20% of the total mass of diol and diisocyanate, and the amount of catalyst used is 3-5% of the total mass of diol, diisocyanate and plant dye; the reaction temperature is 65-75°C, and the reaction time is 90-180min.

[0014] Furthermore, in step S3, the mass ratio of the intermediate to the chain extender is 20-80:4-20, the reaction temperature is 65-75° C., and the reaction time is 60-180 min.

[0015] Furthermore, in step S4, the mass ratio of polyamine, water and ethylenediamine is 2-4:25-45:1-3; the reaction temperature is 40-50° C., and the reaction time is 60-120 min.

[0016] Furthermore, the mass ratio of the chain extender in step S3 to the polyamine in step S4 is 4-20:2-4.

[0017] Furthermore, in step S5, the pre-baking temperature is 80-120°C, and the pre-baking time is 3-8 minutes; the hot pressing temperature is 80-140°C, and the hot pressing time is 90-180 seconds; the aging temperature is 120-140°C, and the aging time is 8-10 minutes.

[0018] Furthermore, in step S5, the substrate includes release paper; the base fabric includes ultrafine fiber needle-punched nonwoven fabric, ultrafine fiber spunlace nonwoven fabric or melt-blown nonwoven fabric; and the thickness of the coating is 0.5 to 1.0 mm.

[0019] Furthermore, natural plants include plants rich in flavonoids;

[0020] The diol includes one or more of polyester diol, polycarbonate diol and polyether diol;

[0021] The diisocyanate includes one or more of isophorone diisocyanate, toluene diisocyanate, hydrogenated phenylmethane diisocyanate, and hexamethylene diisocyanate;

[0022] The catalyst includes an organic bismuth catalyst;

[0023] The chain extender includes one or more of ethylene glycol, diethylene glycol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, diethylene glycol, and glycerol;

[0024] The polyamine includes one or more of diethylenetriamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine and isophoronediamine.

[0025] The present invention also provides natural dye-dyed polyurethane microfiber leather prepared by the method for preparing the natural dye-dyed polyurethane microfiber leather.

[0026] It can be seen from the above technical solution that compared with the prior art, the beneficial effects of the present invention are as follows:

[0027] The preparation method of the polyurethane ultra-fine leather dyed with natural dyes in the present invention is not only a simple physical combination, the method makes the plant dye colored monomers interconnected based on covalent bonds and polyurethane molecular chains through chemical reactions, the process is simpler, the cost is lower, and energy is saved, and the participation of chemical dyes is avoided, and there are advantages such as green environmental protection and no pollution to the environment. And the polyurethane ultra-fine leather dyed with natural dyes prepared by the present invention has a complete color system, bright colors, and high color fastness. More importantly, the plant extract extracted by the present invention contains rich flavonoid compounds, which have strong biological activity and diverse structures, and can give synthetic leather multiple functions such as antibacterial, anti-oxidation and UV protection. DETAILED DESCRIPTION

[0028] The invention provides a method for preparing polyurethane microfiber leather dyed with natural dyes, comprising the following steps:

[0029] S1, immersing natural plants in water for extraction to obtain a plant dye extract, and performing rotary evaporation and freeze drying on the plant dye extract to obtain a plant dye;

[0030] S2, mixing the plant dye, diol, diisocyanate and catalyst and reacting them to obtain an intermediate;

[0031] S3, mixing the intermediate and the chain extender and reacting them to obtain a prepolymer;

[0032] S4, mixing the prepolymer, polyamine, water and ethylenediamine and reacting them to obtain a colored waterborne polyurethane emulsion;

[0033] S5, coating the aqueous polyurethane emulsion on the substrate and pre-baking to form a coating, hot-pressing the coating and the base fabric, and then aging, cooling, peeling, and winding in sequence to obtain natural dye-dyed polyurethane microfiber leather.

[0034] In the present invention, in step S1, the mass volume ratio of natural plants and water is 1g:50-100mL, preferably 1g:60-90mL, and more preferably 1g:70-80mL; the extraction temperature is 30-80°C, preferably 40-70°C, and more preferably 50-60°C; the extraction time is 30-60min, preferably 40-50min, and more preferably 45min.

[0035] In the present invention, in step S1, the pH value of the plant dye extract is 2-12, preferably 4-10, and more preferably 6-8.

[0036] In the present invention, in step S2, the mass ratio of diol to diisocyanate is 3-7:3-7, preferably 4-6:4-6, and more preferably 5:5; the amount of plant dye is 5-20% of the total mass of diol and diisocyanate, preferably 8-16%, and more preferably 10-12%; the amount of catalyst is 3-5% of the total mass of diol, diisocyanate and plant dye, and more preferably 4%; the reaction temperature is 65-75°C, preferably 67-73°C, and more preferably 69-71°C; the reaction time is 90-180min, preferably 100-160min, and more preferably 120-140min.

[0037] In the present invention, in step S3, the mass ratio of the intermediate to the chain extender is 20-80:4-20, preferably 30-60:6-16, and more preferably 40-50:8-12; the reaction temperature is 65-75°C, preferably 67-73°C, and more preferably 69-71°C; the reaction time is 60-180min, preferably 80-160min, and more preferably 100-140min.

[0038] In the present invention, in step S4, the mass ratio of polyamine, water and ethylenediamine is 2-4:25-45:1-3, preferably 3:30-40:2, and more preferably 3:30:2; the reaction temperature is 40-50°C, preferably 42-48°C, and more preferably 44-46°C; the reaction time is 60-120 min, preferably 70-100 min, and more preferably 80-90 min.

[0039] In the present invention, the mass ratio of the chain extender in step S3 to the polyamine in step S4 is 4 to 20:2 to 4, preferably 6 to 16:3, and more preferably 8 to 12:3.

[0040] In the present invention, in the step S5, the pre-baking temperature is 80-120°C, preferably 90-110°C, and more preferably 100°C; the pre-baking time is 3-8min, preferably 4-7min, and more preferably 5-6min; the hot pressing bonding temperature is 80-140°C, preferably 90-130°C, and more preferably 100-120°C; the hot pressing bonding time is 90-180s, preferably 100-160s, and more preferably 120-140s; the aging temperature is 120-140°C, preferably 125-135°C, and more preferably 130°C; the aging time is 8-10min, and preferably 9min.

[0041] In the present invention, in step S5, the substrate includes release paper, and the release paper is preferably flat paper or embossed paper; the base fabric includes ultrafine fiber needle-punched non-woven fabric, ultrafine fiber spunlace non-woven fabric or melt-blown non-woven fabric; the thickness of the coating is 0.5 to 1.0 mm, preferably 0.6 to 0.9 mm, and more preferably 0.7 to 0.8 mm.

[0042] In the present invention, the natural plants include plants rich in flavonoids, preferably lotus leaves, mugwort leaves or sophora japonica seeds;

[0043] The diol includes one or more of polyester diol, polycarbonate diol and polyether diol; the number average molecular weight of the diol is preferably 1500-2500 g / mol, more preferably 2000 g / mol;

[0044] The polyester diol is preferably one or more of polycaprolactone diol, polybutylene succinate diol, polyhexamethylene butylene glycol diol, polyethylene succinate diol, polyhexamethylene ethylene glycol diol, polyethylene terephthalate diol and polybutylene terephthalate diol.

[0045] The polycarbonate diol is preferably one or more of polycarbonate butanediol diol, polycarbonate hexanediol diol, polycarbonate decanediol diol and polycarbonate cyclohexanedimethanol diol;

[0046] The polyether diol is preferably one or more of polytetrahydrofuran diol, polyethylene glycol diol and polypropylene glycol diol;

[0047] The diisocyanate includes one or more of isophorone diisocyanate, toluene diisocyanate, hydrogenated phenylmethane diisocyanate, and hexamethylene diisocyanate;

[0048] The catalyst comprises an organic bismuth catalyst, preferably bismuth 2-ethylhexanoate;

[0049] The chain extender includes one or more of ethylene glycol, diethylene glycol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, diethylene glycol, and glycerol;

[0050] The polyamine includes one or more of diethylenetriamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine and isophoronediamine.

[0051] The present invention also provides natural dye-dyed polyurethane microfiber leather prepared by the method for preparing the natural dye-dyed polyurethane microfiber leather.

[0052] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0053] Example 1

[0054] Take 2.0g of dried lotus leaf leaves, place them in a filter bag and immerse them in 100mL of deionized water for extraction, heat them to 50°C, and extract for 30min, during which the ratio of lotus leaf weight to water volume is maintained at 1g:50mL. After removing the filter bag, filter and obtain the lotus leaf dye extract, adjust the pH of the lotus leaf dye extract to 2, evaporate 60mL of water using a rotary evaporator, and freeze-dry the remaining liquid to obtain the lotus leaf plant dye.

[0055] By weight, 50 parts of polycaprolactone diol (number average molecular weight 2000 g / mol) and 5 parts of vegetable dye were placed in a flask and stirred to mix evenly, and 50 parts of isophorone diisocyanate and 3 parts of bismuth 2-ethylhexanoate catalyst were added to react at 70° C. for 120 minutes to generate an intermediate. Then 4 parts of chain extender ethylene glycol were added and the reaction was continued at 70° C. for 120 minutes to generate a prepolymer.

[0056] The temperature was lowered to 45°C, 2 parts of diethylenetriamine, 25 parts of water and 1 part of ethylenediamine were added, and the mixture was reacted for 90 minutes to obtain a colored waterborne polyurethane emulsion.

[0057] The colored water-based polyurethane emulsion was scraped onto the surface of the flat paper and pre-baked at 100°C for 5 minutes to obtain a coating; then it was laminated with a microfiber needle-punched non-woven fabric at 100°C for 90 seconds; finally, it was aged at 120°C for 8 minutes, cooled to room temperature, and then peeled and rolled to obtain a natural dye-dyed polyurethane microfiber leather.

[0058] Example 2

[0059] The same as Example 1, except that the extraction time is 40 min.

[0060] Example 3

[0061] The same as Example 1, except that the extraction time is 50 min.

[0062] Example 4

[0063] The same as Example 1, except that the amount of the vegetable dye is 10 parts.

[0064] Example 5

[0065] The same as Example 1, except that the amount of the vegetable dye is 15 parts.

[0066] Example 6

[0067] The same as Example 1, except that the lotus leaf is replaced by the sophora japonica seed.

[0068] Example 4

[0069] The same as Example 1, except that the lotus leaf is replaced by the mugwort leaf.

[0070] Comparative Example

[0071] By weight, 50 parts of polycaprolactone diol (number average molecular weight 2000 g / mol), 50 parts of isophorone diisocyanate and 3 parts of bismuth 2-ethylhexanoate catalyst were reacted at 70°C for 120 minutes to generate an intermediate. Then 4 parts of chain extender ethylene glycol were added and the reaction was continued at 70°C for 120 minutes to generate a prepolymer.

[0072] The temperature was lowered to 45°C, 2 parts of diethylenetriamine, 25 parts of water and 1 part of ethylenediamine were added, and the mixture was reacted for 90 minutes to obtain an aqueous polyurethane emulsion.

[0073] The water-based polyurethane emulsion was scraped onto the surface of the flat paper and pre-baked at 100°C for 5 minutes to obtain a coating; then it was laminated with a microfiber needle-punched non-woven fabric base at 100°C for 90 seconds; finally, it was aged at 120°C for 8 minutes, cooled to room temperature, and then peeled and rolled to obtain the polyurethane microfiber leather.

[0074] Performance Testing

[0075] The rubbing color fastness, UV resistance and antibacterial properties of the polyurethane microfiber leathers prepared in Examples 1 to 7 and the comparative example were tested, wherein the rubbing color fastness was tested in accordance with GB / T 29865-2013 "Textiles - Tests for Color Fastness - Rubbing Color Fastness - Small Area Method"; the UV resistance was tested in accordance with GB / T 18830-2009 "Evaluation of UV Protection of Textiles"; the antibacterial property was tested in accordance with GB / T 20944-2008 "Evaluation of Antibacterial Properties of Textiles", and the test results are shown in Table 1.

[0076] Table 1 Performance test results of polyurethane microfiber leather

[0077]

[0078] It can be seen from Table 1 that the performance of colored polyurethane microfiber leather is better than that of colorless polyurethane microfiber leather, and as the amount of natural plant dyes used in the preparation process increases, the ultraviolet protection and antibacterial properties of the microfiber leather are improved. The dry and wet friction fastness of polyurethane microfiber leather dyed with extracts of lotus leaves, wormwood leaves and sophora japonica seeds are both at level 3 or above, and can give polyurethane microfiber leather ultraviolet protection and antibacterial properties.

[0079] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing polyurethane microfiber leather dyed with natural dyes, characterized in that: The following steps are involved: S1, immersing natural plants in water for extraction to obtain a plant dye extract, and performing rotary evaporation and freeze drying on the plant dye extract to obtain a plant dye; S2, mixing the plant dye, diol, diisocyanate and catalyst and reacting them to obtain an intermediate; S3, mixing the intermediate and the chain extender and reacting them to obtain a prepolymer; S4, mixing the prepolymer, polyamine, water and ethylenediamine and reacting them to obtain a colored waterborne polyurethane emulsion; S5, coating the aqueous polyurethane emulsion on the substrate and pre-baking to form a coating, hot-pressing the coating and the base fabric, and then aging, cooling, peeling, and winding in sequence to obtain natural dye-dyed polyurethane microfiber leather.

2. The method for preparing the natural dye-dyed polyurethane microfiber leather according to claim 1, wherein: In the step S1, the mass volume ratio of natural plants to water is 1 g: 50-100 mL; the extraction temperature is 30-80° C., and the extraction time is 30-60 min.

3. The method for preparing the natural dye-dyed polyurethane microfiber leather according to claim 1, characterized in that: In the step S2, the mass ratio of diol to diisocyanate is 3-7:3-7, the amount of plant dye used is 5-20% of the total mass of diol and diisocyanate, and the amount of catalyst used is 3-5% of the total mass of diol, diisocyanate and plant dye; the reaction temperature is 65-75°C, and the reaction time is 90-180min.

4. The method for preparing the natural dye-dyed polyurethane microfiber leather according to claim 2 or 3, characterized in that, In the step S3, the mass ratio of the intermediate to the chain extender is 20-80:4-20, the reaction temperature is 65-75° C., and the reaction time is 60-180 min.

5. The method for preparing the natural dye-dyed polyurethane microfiber leather according to claim 4, characterized in that: In the step S4, the mass ratio of polyamine, water and ethylenediamine is 2-4:25-45:1-3; the reaction temperature is 40-50° C., and the reaction time is 60-120 min.

6. The method for preparing the natural dye-dyed polyurethane microfiber leather according to claim 5, characterized in that: The mass ratio of the chain extender in step S3 to the polyamine in step S4 is 4-20:2-4.

7. The method for preparing the natural dye-dyed polyurethane microfiber leather according to claim 2, 3 or 6, characterized in that: In the step S5, the pre-baking temperature is 80-120° C., and the pre-baking time is 3-8 minutes; the hot pressing temperature is 80-140° C., and the hot pressing time is 90-180 seconds; the aging temperature is 120-140° C., and the aging time is 8-10 minutes.

8. The method for preparing the natural dye-dyed polyurethane microfiber leather according to claim 7, characterized in that: In the step S5, the substrate includes release paper; the base fabric includes ultrafine fiber needle-punched nonwoven fabric, ultrafine fiber spunlace nonwoven fabric or melt-blown nonwoven fabric; and the thickness of the coating is 0.5 to 1.0 mm.

9. The method for preparing the natural dye-dyed polyurethane microfiber leather according to claim 5 or 8, characterized in that: Natural plants include those rich in flavonoids; The diol includes one or more of polyester diol, polycarbonate diol and polyether diol; The diisocyanate includes one or more of isophorone diisocyanate, toluene diisocyanate, hydrogenated phenylmethane diisocyanate, and hexamethylene diisocyanate; The catalyst includes an organic bismuth catalyst; The chain extender includes one or more of ethylene glycol, diethylene glycol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, diethylene glycol, and glycerol; The polyamine includes one or more of diethylenetriamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine and isophoronediamine.

10. Natural dye-dyed polyurethane microfiber leather prepared by the method for preparing natural dye-dyed polyurethane microfiber leather according to any one of claims 1 to 9.