Manufacturing method of golden velvet

The yarn is made by blending high F wire, high shrink wire, mulberry silk and modified in the modified solution of tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene and ethanol, and the gold velvet fabric is solved. The problem of color difficulty achieves higher coloring rate and color fastness, reducing the difficulty of dyeing.

CN118979398APending Publication Date: 2024-11-19HANG ZHOU HUI WEI SHI YONG SHENG RAN ZHENG YOU XIAN GONG SI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411107773.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Gold velvet fabrics have difficulty in coloring during production, which makes them more difficult to dye.

Method used

The yarn is made by blended with high F wire, high shrinkage wire, and mulberry silk, and is modified in a modified solution made of tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene and ethanol to form a concave and convex structure. Improve pigment adhesion and color fastness.

Benefits of technology

It significantly improves the coloring rate and color fastness of gold velvet fabrics, reduces the difficulty of dyeing, and makes the dyed fabric less likely to fade and has better quality.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of textile, and particularly discloses a golden velvet manufacturing method which comprises the following steps: step 1), blending high-F silk, high-shrinkage silk and mulberry silk to obtain yarns; step 2), soaking yarns in the modification liquid for modification, and drying to obtain modified yarns; the method comprises the following steps of (1) preparing modified yarn, (2) preparing modified yarn, (3) weaving the modified yarn into a fabric to obtain a prefabricated fabric, (4) heating and shaping the prefabricated fabric to obtain a shaped fabric, and (5) raising the shaped fabric to obtain the golden velvet fabric, and the modification liquid is a compound of tetraisopropyl titanate, sodium p-styrenesulfonate, diisobutylene and ethanol.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of textiles, and in particular to a method for making golden velvet. Background Art

[0002] Gold velvet fabric is a high-end textile, mainly made of mulberry silk or other artificial silk and viscose rayon. With its unique luster, soft touch and excellent warmth retention, it has become a high-end choice in the fields of clothing and home furnishing. However, gold velvet fabric has the problem of difficulty in coloring during production, which makes it difficult to dye gold velvet fabric, so there is still room for improvement. Summary of the invention

[0003] In order to make the gold velvet fabric easier to color, the present application provides a method for making gold velvet.

[0004] The present application provides a method for producing golden velvet using the following technical solution: A method for making golden velvet comprises the following steps: Step 1), blending high F yarn, high shrinkage yarn and mulberry silk to obtain yarn; Step 2), immersing the yarn in a modifying liquid for modification, and drying to obtain modified yarn; Step 3), weaving the modified yarn into fabric to obtain prefabricated fabric; Step 4), heating and shaping the prefabricated fabric to obtain a shaped fabric; Step 5), raising the shaped fabric to obtain golden velvet fabric; The modified liquid is a compound of tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene and ethanol.

[0005] By adopting the above technical scheme, the yarn is obtained by blending high F silk, high shrinkage silk and mulberry silk, so that the surface of the fabric formed by weaving can produce a concave and convex surface, and the longitudinal depth is increased, so that the pigment is easier to adhere to the fabric and easy to color. After the yarn is modified in a modifying liquid composed of tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene and ethanol, the adhesion of the pigment on the fabric can be further improved, making it easier to color, and the dyed gold velvet is less likely to fade, has higher color fastness and better quality.

[0006] Preferably, the mass ratio of the high F yarn, the high shrinkage yarn and the mulberry silk is 10-15:35-40:45-55.

[0007] By adopting the above technical solution and specifically selecting the mass ratio of high F silk, high shrinkage silk and mulberry silk, the effect of forming a concave and convex surface on the surface of the fabric is more significant, and the velvet fabric is easier to color.

[0008] Preferably, the mass ratio of tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene and ethanol is 3-5:7-9:4-6:100.

[0009] By adopting the above technical scheme and specifically selecting the mass ratio of tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene and ethanol, the modification effect is better, the gold velvet fabric is easier to color, and the color fastness is higher.

[0010] Preferably, the high F yarn is polyester FDY.

[0011] By adopting the above technical solution and specifically selecting polyester POY to better match it with high shrinkage yarn and mulberry silk, the gold velvet fabric is easier to color.

[0012] Preferably, the specification of the high F yarn is 100D / 144F.

[0013] By adopting the above technical solution and specifically selecting 100D / 144F, the combination with high shrinkage silk and mulberry silk is better, the concave and convex surface is better formed, and the coloring effect is better.

[0014] Preferably, the high shrinkage yarn is polyester POY.

[0015] By adopting the above technical solution, by specifically selecting high shrinkage yarn as polyester POY, the effect of combining with high F yarn and mulberry silk is better and it is easier to color.

[0016] Preferably, the specification of the high shrinkage yarn is 75D / 36F.

[0017] By adopting the above technical solution and specifically selecting 75D / 36F, it can be better matched with high F silk and mulberry silk, the longitudinal depth can be better improved, and the problem of coloring difficulty can be better solved.

[0018] Preferably, in the step 4), during heating and setting, the temperature of the fabric setting machine is set to: 60°C for the first section, 90°C for the second section, 100°C for the third section, 110°C for the fourth section, 150°C for the fifth section, and 160°C for the sixth to tenth sections.

[0019] By adopting the above technical solution, the shaping effect is better and the quality of the velvet fabric is better through segmented shaping from low temperature to high temperature.

[0020] In summary, this application has the following beneficial effects: 1. Since the yarn is made by blending high F silk, high shrinkage silk and mulberry silk in the present application, the surface of the fabric formed by weaving can produce a concave and convex surface, thereby increasing the longitudinal depth, so that the pigment is easier to adhere to the fabric and is easy to color. After the yarn is modified in a modified medium composed of tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene and ethanol, the adhesion of the pigment to the fabric can be further improved, making it easier to color, and making the gold velvet less likely to fade, with higher color fastness and better quality.

[0021] 2. In the present application, it is preferred to specifically select the mass ratio of high F silk, high shrinkage silk and mulberry silk so that the effect of forming a concave and convex surface on the surface of the fabric is more significant and the gold velvet fabric is easier to color.

[0022] 3. In the present application, it is preferred to specifically select the mass ratio of tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene and ethanol, so that the modification effect is better, the gold velvet fabric is easier to color, and the color fastness is higher. DETAILED DESCRIPTION

[0023] The present application is further described in detail below with reference to the embodiments.

[0024] Example 1 A method for making golden velvet, characterized in that it comprises the following steps: Step 1), high F yarn, high shrinkage yarn and mulberry silk are blended to obtain yarn, and the mass ratio of high F yarn, high shrinkage yarn and mulberry silk is 10:35:45.

[0025] Step 2), soaking the yarn in the modification liquid, keeping the temperature at 50°C, soaking and modifying for 3 hours, filtering out the yarn, and drying it with hot air at 100°C to obtain the modified yarn. The modification liquid is prepared by uniformly mixing tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene, and ethanol. The mass ratio of tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene, and ethanol is 3:7:4:100.

[0026] Step 3), weaving the modified yarn into fabric through a shuttle loom to obtain a prefabricated fabric.

[0027] Step 4), heating and shaping the prefabricated fabric. During heating and shaping, the temperature of the fabric shaping machine is set to: 60°C for the first section, 90°C for the second section, 100°C for the third section, 110°C for the fourth section, 150°C for the fifth section, and 160°C for the sixth to tenth sections to obtain the shaped fabric.

[0028] Step 5), the shaped fabric is subjected to a raising machine for raising treatment to obtain a velvet fabric.

[0029] The high F yarn is polyester FDY, and the specification is 100D / 144F.

[0030] The high shrinkage yarn is polyester POY with a specification of 75D / 36F.

[0031] The mulberry silk was purchased from Yingkou Meidian Home Textile Co., Ltd., with a fiber length of 38-90mm.

[0032] Tetraisopropyl titanate was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 546-68-9.

[0033] Sodium styrene sulfonate was purchased from Guangzhou Shanghe Chemical Technology Co., Ltd., CAS No.: 2695-37-6.

[0034] Diisobutylene was purchased from Hubei Xingyan New Material Technology Co., Ltd., CAS No.: 107-40-4.

[0035] Ethanol is anhydrous ethanol with a concentration of 95%, which is commercially available.

[0036] Example 2 A method for making golden velvet, characterized in that it comprises the following steps: Step 1), high F yarn, high shrinkage yarn and mulberry silk are blended to obtain yarn, and the mass ratio of high F yarn, high shrinkage yarn and mulberry silk is 13:37:50.

[0037] Step 2), immersing the yarn in the modification liquid, keeping the temperature at 55°C, immersing and modifying for 3.5 hours, filtering out the yarn, and drying it with hot air at 100°C to obtain the modified yarn. The modification liquid is prepared by uniformly mixing tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene, and ethanol, and the mass ratio of tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene, and ethanol is 4:8:5:100.

[0038] Step 3), weaving the modified yarn into fabric through a shuttle loom to obtain a prefabricated fabric.

[0039] Step 4), heating and shaping the prefabricated fabric. During heating and shaping, the temperature of the fabric shaping machine is set to: 60°C for the first section, 90°C for the second section, 100°C for the third section, 110°C for the fourth section, 150°C for the fifth section, and 160°C for the sixth to tenth sections to obtain the shaped fabric.

[0040] Step 5), the shaped fabric is subjected to a raising machine for raising treatment to obtain a velvet fabric.

[0041] The high F yarn is polyester FDY, and the specification is 100D / 144F.

[0042] The high shrinkage yarn is polyester POY with a specification of 75D / 36F.

[0043] The mulberry silk was purchased from Yingkou Meidian Home Textile Co., Ltd., with a fiber length of 38-90mm.

[0044] Tetraisopropyl titanate was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 546-68-9.

[0045] Sodium styrene sulfonate was purchased from Guangzhou Shanghe Chemical Technology Co., Ltd., CAS No.: 2695-37-6.

[0046] Diisobutylene was purchased from Hubei Xingyan New Material Technology Co., Ltd., CAS No.: 107-40-4.

[0047] Ethanol is anhydrous ethanol with a concentration of 95%, which is commercially available.

[0048] Example 3 A method for making golden velvet, characterized in that it comprises the following steps: Step 1), high F yarn, high shrinkage yarn and mulberry silk are blended to obtain yarn, and the mass ratio of high F yarn, high shrinkage yarn and mulberry silk is 15:40:55.

[0049] Step 2), soaking the yarn in the modification liquid, keeping the temperature at 60°C, soaking and modifying for 4 hours, filtering out the yarn, and drying it with hot air at 100°C to obtain the modified yarn. The modification liquid is prepared by uniformly mixing tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene, and ethanol. The mass ratio of tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene, and ethanol is 5:9:6:100.

[0050] Step 3), weaving the modified yarn into fabric through a shuttle loom to obtain a prefabricated fabric.

[0051] Step 4), heating and shaping the prefabricated fabric. During heating and shaping, the temperature of the fabric shaping machine is set to: 60°C for the first section, 90°C for the second section, 100°C for the third section, 110°C for the fourth section, 150°C for the fifth section, and 160°C for the sixth to tenth sections to obtain the shaped fabric.

[0052] Step 5), the shaped fabric is subjected to a raising machine for raising treatment to obtain a velvet fabric.

[0053] The high F yarn is polyester FDY, and the specification is 100D / 144F.

[0054] The high shrinkage yarn is polyester POY with a specification of 75D / 36F.

[0055] The mulberry silk was purchased from Yingkou Meidian Home Textile Co., Ltd., with a fiber length of 38-90mm.

[0056] Tetraisopropyl titanate was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 546-68-9.

[0057] Sodium styrene sulfonate was purchased from Guangzhou Shanghe Chemical Technology Co., Ltd., CAS No.: 2695-37-6.

[0058] Diisobutylene was purchased from Hubei Xingyan New Material Technology Co., Ltd., CAS No.: 107-40-4.

[0059] Ethanol is anhydrous ethanol with a concentration of 95%, which is commercially available.

[0060] Comparative Example 1 A method for making golden velvet, characterized in that it comprises the following steps: Step 1), high F yarn, high shrinkage yarn and mulberry silk are blended to obtain yarn, and the mass ratio of high F yarn, high shrinkage yarn and mulberry silk is 13:37:50.

[0061] Step 2), immersing the yarn in the modification liquid, keeping the temperature at 55°C, immersing and modifying for 3.5 hours, filtering out the yarn, and drying it with hot air at 100°C to obtain the modified yarn. The modification liquid is prepared by uniformly mixing isobutyl triethoxy silane, sodium styrene sulfonate, diisobutylene, and ethanol. The mass ratio of isobutyl triethoxy silane, sodium styrene sulfonate, diisobutylene, and ethanol is 4:8:5:100.

[0062] Step 3), weaving the modified yarn into fabric through a shuttle loom to obtain a prefabricated fabric.

[0063] Step 4), heating and shaping the prefabricated fabric. During heating and shaping, the temperature of the fabric shaping machine is set to: 60°C for the first section, 90°C for the second section, 100°C for the third section, 110°C for the fourth section, 150°C for the fifth section, and 160°C for the sixth to tenth sections to obtain the shaped fabric.

[0064] Step 5), the shaped fabric is subjected to a raising machine for raising treatment to obtain a velvet fabric.

[0065] The high F yarn is polyester FDY, and the specification is 100D / 144F.

[0066] The high shrinkage yarn is polyester POY with a specification of 75D / 36F.

[0067] The mulberry silk was purchased from Yingkou Meidian Home Textile Co., Ltd., with a fiber length of 38-90mm.

[0068] Isobutyltriethoxysilane was purchased from Qufu Yishun Chemical Co., Ltd., CAS No.: 17980-47-1.

[0069] Sodium styrene sulfonate was purchased from Guangzhou Shanghe Chemical Technology Co., Ltd., CAS No.: 2695-37-6.

[0070] Diisobutylene was purchased from Hubei Xingyan New Material Technology Co., Ltd., CAS No.: 107-40-4.

[0071] Ethanol is anhydrous ethanol with a concentration of 95%, which is commercially available.

[0072] Comparative Example 2 A method for making golden velvet, characterized in that it comprises the following steps: Step 1), high F yarn, high shrinkage yarn and mulberry silk are blended to obtain yarn, and the mass ratio of high F yarn, high shrinkage yarn and mulberry silk is 13:37:50.

[0073] Step 2), soaking the yarn in the modification liquid, keeping the temperature at 55°C, soaking and modifying for 3.5 hours, filtering out the yarn, and drying it with hot air at 100°C to obtain the modified yarn. The modification liquid is prepared by uniformly mixing tetraisopropyl titanate, octadecyltrimethylammonium chloride, diisobutylene, and ethanol. The mass ratio of tetraisopropyl titanate, octadecyltrimethylammonium chloride, diisobutylene, and ethanol is 4:8:5:100.

[0074] Step 3), weaving the modified yarn into fabric through a shuttle loom to obtain a prefabricated fabric.

[0075] Step 4), heating and shaping the prefabricated fabric. During heating and shaping, the temperature of the fabric shaping machine is set to: 60°C for the first section, 90°C for the second section, 100°C for the third section, 110°C for the fourth section, 150°C for the fifth section, and 160°C for the sixth to tenth sections to obtain the shaped fabric.

[0076] Step 5), the shaped fabric is subjected to a raising machine for raising treatment to obtain a velvet fabric.

[0077] The high F yarn is polyester FDY, and the specification is 100D / 144F.

[0078] The high shrinkage yarn is polyester POY with a specification of 75D / 36F.

[0079] The mulberry silk was purchased from Yingkou Meidian Home Textile Co., Ltd., with a fiber length of 38-90mm.

[0080] Tetraisopropyl titanate was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 546-68-9.

[0081] Octadecyltrimethylammonium chloride was purchased from Shandong Anmi Chemical Technology Co., Ltd., CAS No.: 112-03-8.

[0082] Diisobutylene was purchased from Hubei Xingyan New Material Technology Co., Ltd., CAS No.: 107-40-4.

[0083] Ethanol is anhydrous ethanol with a concentration of 95%, which is commercially available.

[0084] Comparative Example 3 A method for making golden velvet, characterized in that it comprises the following steps: Step 1), high F yarn, high shrinkage yarn and mulberry silk are blended to obtain yarn, and the mass ratio of high F yarn, high shrinkage yarn and mulberry silk is 13:37:50.

[0085] Step 2), immersing the yarn in the modification liquid, keeping the temperature at 55°C, immersing and modifying for 3.5 hours, filtering out the yarn, and drying it with hot air at 100°C to obtain the modified yarn. The modification liquid is prepared by uniformly mixing tetraisopropyl titanate, sodium styrene sulfonate, ethyl orthosilicate, and ethanol. The mass ratio of tetraisopropyl titanate, sodium styrene sulfonate, ethyl orthosilicate, and ethanol is 4:8:5:100.

[0086] Step 3), weaving the modified yarn into fabric through a shuttle loom to obtain a prefabricated fabric.

[0087] Step 4), heating and shaping the prefabricated fabric. During heating and shaping, the temperature of the fabric shaping machine is set to: 60°C for the first section, 90°C for the second section, 100°C for the third section, 110°C for the fourth section, 150°C for the fifth section, and 160°C for the sixth to tenth sections to obtain the shaped fabric.

[0088] Step 5), the shaped fabric is subjected to a raising machine for raising treatment to obtain a velvet fabric.

[0089] The high F yarn is polyester FDY, and the specification is 100D / 144F.

[0090] The high shrinkage yarn is polyester POY with a specification of 75D / 36F.

[0091] The mulberry silk was purchased from Yingkou Meidian Home Textile Co., Ltd., with a fiber length of 38-90mm.

[0092] Tetraisopropyl titanate was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 546-68-9.

[0093] Sodium styrene sulfonate was purchased from Guangzhou Shanghe Chemical Technology Co., Ltd., CAS No.: 2695-37-6.

[0094] Tetraethyl orthosilicate was purchased from Shandong Poly Chemical Co., Ltd., CAS No.: 78-10-4.

[0095] Ethanol is anhydrous ethanol with a concentration of 95%, which is commercially available.

[0096] Comparative Example 4 A method for making golden velvet, characterized in that it comprises the following steps: Step 1), high F yarn, high shrinkage yarn and mulberry silk are blended to obtain yarn, and the mass ratio of high F yarn, high shrinkage yarn and mulberry silk is 13:37:50.

[0097] Step 2), soaking the yarn in the modification liquid, keeping the temperature at 55°C, soaking and modifying for 3.5 hours, filtering out the yarn, and drying it with hot air at 100°C to obtain the modified yarn. The modification liquid is prepared by uniformly mixing isobutyl triethoxysilane, octadecyl trimethyl ammonium chloride, tetraethyl orthosilicate, and ethanol. The mass ratio of isobutyl triethoxysilane, octadecyl trimethyl ammonium chloride, tetraethyl orthosilicate, and ethanol is 4:8:5:100.

[0098] Step 3), weaving the modified yarn into fabric through a shuttle loom to obtain a prefabricated fabric.

[0099] Step 4), heating and shaping the prefabricated fabric. During heating and shaping, the temperature of the fabric shaping machine is set to: 60°C for the first section, 90°C for the second section, 100°C for the third section, 110°C for the fourth section, 150°C for the fifth section, and 160°C for the sixth to tenth sections to obtain the shaped fabric.

[0100] Step 5), the shaped fabric is subjected to a raising machine for raising treatment to obtain a velvet fabric.

[0101] The high F yarn is polyester FDY, and the specification is 100D / 144F.

[0102] The high shrinkage yarn is polyester POY with a specification of 75D / 36F.

[0103] The mulberry silk was purchased from Yingkou Meidian Home Textile Co., Ltd., with a fiber length of 38-90mm.

[0104] Isobutyltriethoxysilane was purchased from Qufu Yishun Chemical Co., Ltd., CAS No.: 17980-47-1.

[0105] Octadecyltrimethylammonium chloride was purchased from Shandong Anmi Chemical Technology Co., Ltd., CAS No.: 112-03-8.

[0106] Tetraethyl orthosilicate was purchased from Shandong Poly Chemical Co., Ltd., CAS No.: 78-10-4.

[0107] Ethanol is anhydrous ethanol with a concentration of 95%, which is commercially available.

[0108] Comparative Example 5 A method for making golden velvet, characterized in that it comprises the following steps: Step 1), high F yarn, high shrinkage yarn and mulberry silk are blended to obtain yarn, and the mass ratio of high F yarn, high shrinkage yarn and mulberry silk is 5:55:40.

[0109] Step 2), immersing the yarn in the modification liquid, keeping the temperature at 55°C, immersing and modifying for 3.5 hours, filtering out the yarn, and drying it with hot air at 100°C to obtain the modified yarn. The modification liquid is prepared by uniformly mixing tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene, and ethanol, and the mass ratio of tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene, and ethanol is 4:8:5:100.

[0110] Step 3), weaving the modified yarn into fabric through a shuttle loom to obtain a prefabricated fabric.

[0111] Step 4), heating and shaping the prefabricated fabric. During heating and shaping, the temperature of the fabric shaping machine is set to: 60°C for the first section, 90°C for the second section, 100°C for the third section, 110°C for the fourth section, 150°C for the fifth section, and 160°C for the sixth to tenth sections to obtain the shaped fabric.

[0112] Step 5), the shaped fabric is subjected to a raising machine for raising treatment to obtain a velvet fabric.

[0113] The high F yarn is polyester FDY, and the specification is 100D / 144F.

[0114] The high shrinkage yarn is polyester POY with a specification of 75D / 36F.

[0115] The mulberry silk was purchased from Yingkou Meidian Home Textile Co., Ltd., with a fiber length of 38-90mm.

[0116] Tetraisopropyl titanate was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 546-68-9.

[0117] Sodium styrene sulfonate was purchased from Guangzhou Shanghe Chemical Technology Co., Ltd., CAS No.: 2695-37-6.

[0118] Diisobutylene was purchased from Hubei Xingyan New Material Technology Co., Ltd., CAS No.: 107-40-4.

[0119] Ethanol is anhydrous ethanol with a concentration of 95%, which is commercially available.

[0120] Comparative Example 6 A method for making golden velvet, characterized in that it comprises the following steps: Step 1), high F yarn, high shrinkage yarn and mulberry silk are blended to obtain yarn, and the mass ratio of high F yarn, high shrinkage yarn and mulberry silk is 25:5:70.

[0121] Step 2), immersing the yarn in the modification liquid, keeping the temperature at 55°C, immersing and modifying for 3.5 hours, filtering out the yarn, and drying it with hot air at 100°C to obtain the modified yarn. The modification liquid is prepared by uniformly mixing tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene, and ethanol, and the mass ratio of tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene, and ethanol is 4:8:5:100.

[0122] Step 3), weaving the modified yarn into fabric through a shuttle loom to obtain a prefabricated fabric.

[0123] Step 4), heating and shaping the prefabricated fabric. During heating and shaping, the temperature of the fabric shaping machine is set to: 60°C for the first section, 90°C for the second section, 100°C for the third section, 110°C for the fourth section, 150°C for the fifth section, and 160°C for the sixth to tenth sections to obtain the shaped fabric.

[0124] Step 5), the shaped fabric is subjected to a raising machine for raising treatment to obtain a velvet fabric.

[0125] The high F yarn is polyester FDY, and the specification is 100D / 144F.

[0126] The high shrinkage yarn is polyester POY with a specification of 75D / 36F.

[0127] The mulberry silk was purchased from Yingkou Meidian Home Textile Co., Ltd., with a fiber length of 38-90mm.

[0128] Tetraisopropyl titanate was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 546-68-9.

[0129] Sodium styrene sulfonate was purchased from Guangzhou Shanghe Chemical Technology Co., Ltd., CAS No.: 2695-37-6.

[0130] Diisobutylene was purchased from Hubei Xingyan New Material Technology Co., Ltd., CAS No.: 107-40-4.

[0131] Ethanol is anhydrous ethanol with a concentration of 95%, which is commercially available.

[0132] Experiment 1 Coloring rate detection The coloring rate F (%) of the golden velvet of each embodiment and comparative example was tested according to GB / T 9337-2009 “Determination of the coloring rate of disperse dyes at high temperature”.

[0133] The dye was purchased from Shanghai Mengdihu Industrial Co., Ltd., item number JFY.

[0134] Add 10 kg of dye into 100 kg of water and stir evenly to obtain the dyeing solution.

[0135] The dyeing conditions were 80°C, dyeing for 30 minutes, and sampling and testing were performed.

[0136] Experiment 2 According to GB / T42223-2022 "Textiles - Tests for Color Fastness - Color Fastness to Rubbing - Gakushin Method", the staining levels of the test samples made after dyeing the golden velvet in each embodiment and comparative example were tested.

[0137] The dye was purchased from Shanghai Mengdihu Industrial Co., Ltd., item number JFY.

[0138] The dyeing process is as follows: In 100kg of water, add 10kg of dye and stir evenly to obtain a dyeing solution. Then heat the dyeing solution to 80°C, soak the gold velvet fabric in the dyeing solution for 30 minutes, filter out the dyeing solution, rinse with clean water until the washing water is colorless, and dry it to obtain the dyed gold velvet test sample.

[0139] The friction test condition is dry friction.

[0140] The specific experimental data of Experiments 1 and 2 are shown in Table 1.

[0141] Table 1 Coloring rate F(%) Color staining degree Example 1 92.3 4-5 Example 2 93.5 4-5 Example 3 92.9 4-5 Comparative Example 1 68.5 2-3 Comparative Example 2 71.8 3-4 Comparative Example 3 66.3 2-3 Comparative Example 4 64.7 2-3 Comparative Example 5 81.6 4-5 Comparative Example 6 76.2 4-5 According to the data comparison in Table 1, the coloring rate and color fastness of each embodiment are significantly higher than those of the comparative examples. It can be seen that when the yarn is modified by the modifying liquid formed by compounding tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene and ethanol, the coloring rate can be significantly improved, the dyeing difficulty can be reduced, and it is not easy to fade after dyeing, and the quality is better.

[0142] Although the yarns were also modified in Comparative Examples 1-4, the modified effect was relatively general due to the destruction of the compound system of tetraisopropyl titanate, sodium styrene sulfonate and diisobutylene. The effect of improving the coloring rate and color fastness was relatively general, which was significantly lower than that of the embodiments.

[0143] In Comparative Examples 5-6, since the mass ratio of high F yarn, high shrinkage yarn and mulberry silk was changed, even though the yarn was modified in a modification liquid prepared by tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene and ethanol, the coloring rate was still lower than that of the various embodiments. It can be seen that in each embodiment, high F yarn, high shrinkage yarn and mulberry silk are blended into yarn in a specific ratio, which helps to improve the coloring rate and reduce the difficulty of dyeing.

[0144] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A method for making golden velvet, characterized in that: The following steps are involved: Step 1), blending high F yarn, high shrinkage yarn and mulberry silk to obtain yarn; Step 2), the yarn is immersed in a modifying liquid for modification, and then dried to obtain a modified yarn; Step 3), weaving the modified yarn into fabric to obtain prefabricated fabric; Step 4), heating and shaping the prefabricated fabric to obtain a shaped fabric; Step 5), performing a raising process on the shaped fabric to obtain a velvet fabric; The modified liquid is a compound of tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene and ethanol.

2. The method for making golden velvet according to claim 1, characterized in that: The mass ratio of the high F yarn, the high shrinkage yarn and the mulberry silk is 10-15:35-40:45-55.

3. The method for making golden velvet according to claim 2, characterized in that: The mass ratio of tetraisopropyl titanate, sodium styrene sulfonate, diisobutylene and ethanol is 3-5:7-9:4-6:

100.

4. The method for making golden velvet according to claim 2, characterized in that: The high F yarn is polyester FDY.

5. The method for making golden velvet according to claim 4, characterized in that: The specification of the high F wire is 100D / 144F.

6. The method for making golden velvet according to claim 2, characterized in that: The high shrinkage yarn is polyester POY.

7. The method for making golden velvet according to claim 6, characterized in that: The specification of the high shrinkage yarn is 75D / 36F.

8. The method for making golden velvet according to claim 1, characterized in that: In the step 4), during heating and setting, the temperature of the fabric setting machine is set to: 60°C for the first section, 90°C for the second section, 100°C for the third section, 110°C for the fourth section, 150°C for the fifth section, and 160°C for the sixth to tenth sections.