High-resilience synthetic leather and preparation method thereof

Through multi-layer structural design and specific raw material formula, the elasticity and comfort of synthetic leather are improved, and the problems of low elasticity and thick fiber structure of existing synthetic leather are solved, achieving higher rebound performance and better fit for genuine leather Natural texture effect.

CN118932740APending Publication Date: 2024-11-12TIANSHOU FUJIAN SUPERFIBER TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410842892.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing synthetic leather has low elasticity, thick fiber structure, and is not delicate enough, which makes it impossible to better adapt to human movement when wearing it and the experience is not comfortable enough.

Method used

Highly resilient synthetic leather design with multi-layer structures, including fabric layers, tear-resistant layers, substrate layers and backing layers, improves the resilience and comfort of synthetic leather through specific raw material formulations and process flows, such as using Diisocyanate, polyester polyol, amine curing agent and other materials form a fabric layer, high-strength polyester fiber and mesh cloth form a tear-resistant layer, and EVA, crosslinking agent, polycarbon polyurethane resin and other materials form a base material The layer is reduced by washing and baking steps.

Benefits of technology

It improves the rebound performance and comfort of synthetic leather, making it more suitable for the natural texture of genuine leather, softer, can better adapt to human movement and provide a better wearing experience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932740A_ABST
    Figure CN118932740A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of synthetic leather, and discloses high-resilience synthetic leather and a preparation method thereof.The high-resilience synthetic leather comprises a fabric layer, and the fabric layer is used for protecting the synthetic leather; the anti-tearing layer is used for providing the strength and durability of the synthetic leather and preventing tearing or damage in the using process, the base material layer serves as a main component of the synthetic leather, and the base material layer determines the basic performance and texture of the synthetic leather; and the back lining layer is used for enhancing the softness and comfort of the synthetic leather and providing additional functions. According to the high-resilience synthetic leather, the polyurethane resin and other materials are added into the synthetic leather to prepare the high-resilience synthetic leather, so that the synthetic leather has higher resilience, can better adapt to human body movement and provide more comfortable wearing experience, meanwhile, the fiber structure of the synthetic leather is very fine and smooth, and the synthetic leather better fits natural textures of genuine leather in appearance; meanwhile, the fabric is softer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of synthetic leather, in particular to a high-elasticity synthetic leather and a preparation method thereof. Background Art

[0002] Synthetic leather is a man-made material that imitates the appearance and texture of natural leather and is widely used in various fields. With the advancement of technology, the synthetic leather industry has developed dry-process synthetic leather, wet-process synthetic leather and other process technologies, and has used water-based polyurethane technology in the fields of clothing leather, sofa leather, etc. to make synthetic leather suitable for high-end products, injecting new vitality into China's synthetic leather industry.

[0003] In summary, synthetic leather is a man-made material composed of synthetic fibers, plastic resins and other chemical additives, which has a similar appearance and texture to natural leather and is widely used in various fields. With the advancement of technology and the improvement of environmental protection requirements, the synthetic leather industry is developing in a more environmentally friendly and healthy direction.

[0004] The resilience of current synthetic leather is usually low, and the fiber structure of synthetic leather is usually coarse and not delicate enough, so that it cannot better adapt to human body movements when manufactured and worn, resulting in an uncomfortable wearing experience. Summary of the invention

[0005] In view of the fact that the resilience of the above-mentioned existing synthetic leather is usually low, and the fiber structure of the synthetic leather is usually coarse and not delicate enough, so that it cannot better adapt to human body movements when worn, resulting in an uncomfortable wearing experience, the present invention is proposed.

[0006] Therefore, the purpose of the present invention is to provide a high-resilience synthetic leather, and its purpose is to: manufacture a high-resilience synthetic leather so that the synthetic leather has higher resilience performance, can better adapt to human body movement, and provide a more comfortable wearing experience. At the same time, its fiber structure is very delicate, and the appearance is more in line with the natural texture of genuine leather, and it is also softer.

[0007] In order to solve the above technical problems, the present invention provides the following technical solutions: a high resilience synthetic leather, comprising a fabric layer, the fabric layer is used to protect the synthetic leather; an anti-tear layer, the anti-tear layer is used to provide strength and durability to the synthetic leather to prevent tearing or breakage during use; a substrate layer, the substrate layer is the main component of the synthetic leather, and the substrate layer determines the basic performance and texture of the synthetic leather; and a backing layer, the backing layer is used to enhance the softness and comfort of the synthetic leather and provide additional functions.

[0008] As a preferred embodiment of the high resilience synthetic leather of the present invention, the raw material formula of the fabric layer consists of the following components: 6-8 parts of diisocyanate, 5-9 parts of polyester polyol, and 3-6 parts of amine curing agent. All the raw materials are mixed and then coated, and cured into a film at a temperature of 130-140°C.

[0009] As a preferred embodiment of the high resilience synthetic leather of the present invention, the tear-resistant layer is composed of high-strength polyester fibers, yarns and mesh cloth.

[0010] As a preferred embodiment of the high resilience synthetic leather described in the present invention, the raw material formula of the substrate layer is composed of the following components: 5-10 parts of EVA, 15-20 parts of auxiliary cross-linking agent TAI C, 3-6 parts of colorant black masterbatch, 30-60 parts of colorant black masterbatch, polycarbonate type polyurethane resin, and 5-10 parts of dimethyl formyl.

[0011] As a preferred solution of the high resilience synthetic leather of the present invention, the raw material formula of the backing layer consists of the following components: 30-60 parts of polyurethane resin, 2-5 parts of curing agent, and 0.5-2 parts of leveling agent.

[0012] To achieve the above object, the present invention provides the following technical solution: a method for preparing high resilience synthetic leather, comprising the following steps:

[0013] S1, firstly mix all the raw materials of the fabric layer and then apply them, and then cure them into a film at a temperature of 130-140°C to form a fabric layer;

[0014] S2, then coating all the raw materials of the tear-resistant layer on the fabric layer prepared in S1, and curing them into a film at 130-140° C. to form a new tear-resistant layer;

[0015] S3, mixing all raw materials of the substrate layer to prepare a mixture, coating the mixture on the new tear-resistant layer prepared in S2, and curing the mixture at 130-140° C. to form a film to form a new substrate layer;

[0016] S4, then all the raw materials of the backing layer are mixed to form a mixture, the mixture is coated on the new base material layer prepared in S3, cured at 130-140° C. to form a new backing layer and bonded to the base fabric, and dried at 150-165° C. to form a semi-finished synthetic leather;

[0017] S5, washing the semi-finished synthetic leather with water for 8 times, so that the residual concentration of dimethylformamide in the semi-finished synthetic leather is reduced to 10-20%; then washing with water for 4 times, so that the residual concentration of dimethylformamide in the semi-finished synthetic leather is reduced to 5-10%; and finally washing with water for 2 times, so that the residual concentration of dimethylformamide in the semi-finished synthetic leather is reduced to 0%;

[0018] S6, then put the semi-finished synthetic leather into a baking device, control the baking temperature to 120°C for the first time, control the baking temperature to 155°C for the second to fourth times, and control the oven temperature to 130°C for the fifth time until it is completely dried, so as to obtain a high resilience synthetic leather.

[0019] The beneficial effects of the present invention are as follows: the high-resilience synthetic leather made by adding materials such as polyurethane resin to synthetic leather has higher resilience performance, can better adapt to human body movements, and provides a more comfortable wearing experience. At the same time, its fiber structure is very delicate, and its appearance is more in line with the natural texture of genuine leather, and it is also softer. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:

[0021] Figure 1 It is a schematic diagram of a partially cutaway three-dimensional structure of the high resilience synthetic leather of the present invention.

[0022] Description of reference numerals:

[0023] 1. Fabric layer; 2. Tear-resistant layer; 3. Base material layer; 4. Backing layer. DETAILED DESCRIPTION

[0024] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the accompanying drawings.

[0025] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0026] Example 1

[0027] Reference Figure 1 , which is the first embodiment of the present invention, provides a high resilience synthetic leather, the high resilience synthetic leather comprises a fabric layer 1, the fabric layer 1 is used to protect the synthetic leather;

[0028] The tear-resistant layer 2 is used to provide strength and durability to the synthetic leather and prevent tearing or damage during use;

[0029] Base material layer 3, as the main component of synthetic leather, the base material layer determines the basic performance and texture of synthetic leather;

[0030] The backing layer 4 is used to enhance the softness and comfort of the synthetic leather and provide additional functions.

[0031] The raw material formula of the fabric layer 1 consists of the following components: 6 parts of diisocyanate, 5 parts of polyester polyol, and 3 parts of amine curing agent. All the raw materials are mixed and then coated, and cured at a temperature of 130° C. to form a film.

[0032] The tear-resistant layer 2 is composed of high-strength polyester fibers, yarns and mesh cloth.

[0033] The raw material formula of the substrate layer 3 consists of the following components: 5 parts of EVA, 15 parts of the co-crosslinking agent TAI C, 3 parts of the colorant black masterbatch, 30 parts of the polycarbonate polyurethane resin, and 5 parts of dimethylformamide.

[0034] The raw material formula of the backing layer 4 consists of the following components: 30 parts of polyurethane resin, 2 parts of curing agent, and 0.5 parts of leveling agent.

[0035] A method for preparing high resilience synthetic leather comprises the following steps:

[0036] S1, firstly mix all the raw materials of the fabric layer 1 and then apply them, and then cure them into a film at a temperature of 130° C. to form the fabric layer 1;

[0037] S2, then coating all the raw materials of the tear-resistant layer 2 on the fabric layer 1 prepared in S1, and curing them at 130° C. to form a new tear-resistant layer 2;

[0038] S3, mixing all raw materials of the substrate layer 3 to prepare a mixture, coating the mixture on the new tear-resistant layer 2 prepared in S2, and curing it at 130° C. to form a film, thereby forming a new substrate layer 3;

[0039] S4, then all the raw materials of the backing layer 4 are mixed to form a mixture, and the mixture is coated on the new base material layer 3 prepared in S3, and cured at 130°C to form a film to form a new backing layer 4 and bonded to the base fabric, and dried at 150°C to form a semi-finished synthetic leather;

[0040] S5, washing the semi-finished synthetic leather with water for 8 times, so that the residual concentration of dimethylformamide in the semi-finished synthetic leather is reduced to 10-20%; then washing with water for 4 times, so that the residual concentration of dimethylformamide in the semi-finished synthetic leather is reduced to 5-10%; and finally washing with water for 2 times, so that the residual concentration of dimethylformamide in the semi-finished synthetic leather is reduced to 0%;

[0041] S6, then put the semi-finished synthetic leather into a baking device, control the baking temperature to 120°C for the first time, control the baking temperature to 155°C for the second to fourth times, and control the oven temperature to 130°C for the fifth time until it is completely dried, so as to obtain a high resilience synthetic leather.

[0042] Example 2

[0043] The preparation method of Example 2 is basically the same as that of Example 1, except that:

[0044] The raw material formula of the fabric layer 1 consists of the following components: 7 parts of diisocyanate, 7 parts of polyester polyol, and 4 parts of amine curing agent. All the raw materials are mixed and then coated, and cured at a temperature of 130° C. to form a film.

[0045] The raw material formula of the substrate layer 3 consists of the following components: 8 parts of EVA, 17 parts of the co-crosslinking agent TAI C, 4 parts of the colorant black masterbatch, 45 parts of the polycarbonate polyurethane resin, and 8 parts of dimethylformamide.

[0046] The tear-resistant layer 2 is composed of high-strength polyester fibers, yarns and mesh cloth.

[0047] The raw material formula of the backing layer 4 consists of the following components: 45 parts of polyurethane resin, 4 parts of curing agent, and 1.5 parts of leveling agent.

[0048] A method for preparing high resilience synthetic leather comprises the following steps:

[0049] S1, firstly mix all the raw materials of the fabric layer 1 and then apply them, and then cure them into a film at a temperature of 130° C. to form the fabric layer 1;

[0050] S2, then coating all the raw materials of the tear-resistant layer 2 on the fabric layer 1 prepared in S1, and curing them at 130° C. to form a new tear-resistant layer 2;

[0051] S3, mixing all raw materials of the substrate layer 3 to prepare a mixture, coating the mixture on the new tear-resistant layer 2 prepared in S2, and curing it at 130-140° C. to form a film, thereby forming a new substrate layer 3;

[0052] S4, then all the raw materials of the backing layer 4 are mixed to form a mixture, and the mixture is coated on the new base material layer 3 prepared in S3, and cured at 130°C to form a film to form a new backing layer 4 and bonded to the base fabric, and dried at 150°C to form a semi-finished synthetic leather;

[0053] S5, washing the semi-finished synthetic leather with water for 8 times, so that the residual concentration of dimethylformamide in the semi-finished synthetic leather is reduced to 10-20%; then washing with water for 4 times, so that the residual concentration of dimethylformamide in the semi-finished synthetic leather is reduced to 5-10%; and finally washing with water for 2 times, so that the residual concentration of dimethylformamide in the semi-finished synthetic leather is reduced to 0%;

[0054] S6, then put the semi-finished synthetic leather into the baking equipment, control the baking temperature to 120°C for the first time, control the baking temperature to 155°C for the second to fourth times, and control the oven temperature to 130°C for the fifth time until it is completely dried, and then obtain the high resilience synthetic leather

[0055] Example 3

[0056] The preparation method of Example 2 is basically the same as that of the previous example, except that:

[0057] The raw material formula of the fabric layer 1 consists of the following components: 8 parts of diisocyanate, 9 parts of polyester polyol, and 6 parts of amine curing agent. All the raw materials are mixed and then coated, and cured at a temperature of 130° C. to form a film.

[0058] The raw material formula of the substrate layer 3 consists of the following components: 10 parts of EVA, 20 parts of the co-crosslinking agent TAI C, 6 parts of the colorant black masterbatch, 60 parts of the colorant black masterbatch, 10 parts of the polycarbonate polyurethane resin, and 10 parts of dimethylformamide.

[0059] The tear-resistant layer 2 is composed of high-strength polyester fibers, yarns and mesh cloth.

[0060] The raw material formula of the backing layer 4 consists of the following components: 60 parts of polyurethane resin, 5 parts of curing agent, and 2 parts of leveling agent.

[0061] A method for preparing high resilience synthetic leather comprises the following steps:

[0062] S1, firstly mix all the raw materials of the fabric layer 1 and then apply them, and then cure them into a film at a temperature of 140° C. to form the fabric layer 1;

[0063] S2, then coating all the raw materials of the tear-resistant layer 2 on the fabric layer 1 prepared in S1, and curing them into a film at 130-140° C. to form a new tear-resistant layer 2;

[0064] S3, mixing all raw materials of the substrate layer 3 to prepare a mixture, coating the mixture on the new tear-resistant layer 2 prepared in S2, and curing it at 140° C. to form a film, thereby forming a new substrate layer 3;

[0065] S4, then all the raw materials of the backing layer 4 are mixed to form a mixture, and the mixture is coated on the new base material layer 3 prepared in S3, and cured at 140°C to form a film to form a new backing layer 4 and bonded to the base fabric, and dried at 165°C to form a semi-finished synthetic leather;

[0066] S5, washing the semi-finished synthetic leather 10 times to reduce the residual concentration of dimethylformamide in the semi-finished synthetic leather to 10-20%; then washing it 8 times to reduce the residual concentration of dimethylformamide in the semi-finished synthetic leather to 5-10%; and finally washing it 4 times to reduce the residual concentration of dimethylformamide in the semi-finished synthetic leather to 0%;

[0067] S6, then put the semi-finished synthetic leather into the baking equipment, control the baking temperature to 120°C for the first time, control the baking temperature to 155°C for the second to fourth times, and control the oven temperature to 130°C for the fifth time until it is completely dried, and then obtain the high resilience synthetic leather

[0068] The synthetic leather prepared in Examples 1-3 was tested. The resilience test was conducted using a commercially available thickness meter, and the softness test was conducted using a commercially available softness instrument. The test performance is shown in the following table:

[0069] Thickness(mm) Density (kg / m3) Softness(0.1mm) Example 1 0.6 0.55 3 Example 2 0.7 0.45 5 Example 3 0.8 0.43 8

[0070] It can be seen from the experimental data of Examples 1-3 that the softness in Example 3 is the greatest, and thus the elastic effect is better, so that the high resilience synthetic leather made by adding materials such as polyurethane resin to synthetic leather of the present invention has higher resilience performance, can better adapt to human movement, and provide a more comfortable wearing experience. At the same time, its fiber structure is very delicate, and its appearance is more in line with the natural texture of genuine leather, and it is also softer.

[0071] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A high resilience synthetic leather, characterized in that: include: A fabric layer (1), wherein the fabric layer (1) is used to protect the synthetic leather; An anti-tear layer (2), the anti-tear layer (2) is used to provide strength and durability to the synthetic leather and prevent tearing or damage during use; A substrate layer (3), the substrate layer (3) being a main component of the synthetic leather, and determining the basic performance and texture of the synthetic leather; The backing layer (4) is used to enhance the softness and comfort of the synthetic leather and provide additional functions.

2. The high resilience synthetic leather according to claim 1, characterized in that: The raw material formula of the fabric layer (1) consists of the following components: 6-8 parts of diisocyanate, 5-9 parts of polyester polyol, and 3-6 parts of amine curing agent. All the raw materials are mixed and then coated, and cured at a temperature of 130-140° C. to form a film.

3. The high resilience synthetic leather according to claim 2, characterized in that: The tear-resistant layer (2) is composed of high-strength polyester fibers, yarns and mesh cloth.

4. The high resilience synthetic leather according to claim 3, characterized in that: The raw material formula of the substrate layer (3) consists of the following components: 5-10 parts of EVA, 15-20 parts of auxiliary cross-linking agent TAIC, 3-6 parts of colorant black masterbatch, 30-60 parts of polycarbonate polyurethane resin, and 5-10 parts of dimethylformamide.

5. The high resilience synthetic leather according to claim 4, characterized in that: The raw material formula of the backing layer (4) consists of the following components: 30-60 parts of polyurethane resin, 2-5 parts of curing agent, and 0.5-2 parts of leveling agent.

6. A method for preparing a high resilience synthetic leather, which is applied to the high resilience synthetic leather as claimed in claim 5, characterized in that: The following steps are included: S1, firstly mixing all the raw materials of the fabric layer (1) and then coating them, and curing them into a film at a temperature of 130-140° C. to form the fabric layer (1); S2, then coating all the raw materials of the tear-resistant layer (2) on the fabric layer (1) prepared in S1, and curing at 130-140° C. to form a film, thereby forming a new tear-resistant layer (2); S3, mixing all raw materials of the substrate layer (3) to prepare a mixture, coating the mixture on the new tear-resistant layer (2) prepared in S2, and curing the mixture at 130-140° C. to form a film, thereby forming a new substrate layer (3); S4, then all the raw materials of the backing layer (4) are mixed to form a mixture, the mixture is coated on the new base material layer (3) prepared in S3, cured at 130-140° C. to form a new backing layer (4) and bonded to the base fabric, and dried at 150-165° C. to form a semi-finished synthetic leather; S5, washing the semi-finished synthetic leather with water for 8 times, so that the residual concentration of dimethylformamide in the semi-finished synthetic leather is reduced to 10-20%; then washing with water for 4 times, so that the residual concentration of dimethylformamide in the semi-finished synthetic leather is reduced to 5-10%; and finally washing with water for 2 times, so that the residual concentration of dimethylformamide in the semi-finished synthetic leather is reduced to 0%; S6, then put the semi-finished synthetic leather into a baking device, control the baking temperature to 120°C for the first time, control the baking temperature to 155°C for the second to fourth times, and control the oven temperature to 130°C for the fifth time until it is completely dried, so as to obtain a high resilience synthetic leather.