Preparation method of double-process mirror-surface high-transmittance crystal leather
Through the dual process technology combined with dry bonding and semi-dry patching technology, the problem that traditional artificial leather is difficult to improve gloss, transparency and touch at the same time is solved, and a high-transparent crystal leather with crystal luster, transparency and three-dimensional patterns is prepared to meet the high-end Market demand and exhibit excellent wear and fold resistance.
Patent Information
- Application Number
- CN202411308433.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional artificial leather preparation methods are difficult to ensure high gloss, high transparency and high-quality touch at the same time, and are prone to defects such as needle eyes and bubbles.
The preparation method of double-process mirrored high-permeability crystal leather includes one process and two process steps. One process is to scrape and dry multi-layer polyurethane slurry on the pattern release paper to form pearlescent leather semi-finished products; the second process is to coat and dry polyurethane colorless slurry on the mirror release paper to combine lamination pressure Roller technology realizes mirror bonding and peeling to form a finished product of high-permeability crystal leather.
The high-transparent crystal leather produced has significant crystal luster, high transparency, three-dimensional texture, no needle eyes and bubbles, bright colors and smooth surface touch, meeting the demand of the high-end market, and has excellent wear and fold resistance.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field, and in particular to a method for preparing a dual-process mirror-surface high-transmittance crystal leather. Background Art
[0002] At present, there are many artificial leather manufacturing technologies on the market, but the artificial leather prepared by traditional methods still needs to be improved in terms of gloss, transparency, three-dimensional texture and touch. In order to meet the market demand for high-quality artificial leather, new preparation technologies are constantly emerging. The existing technology usually adopts a single dry or wet process to prepare artificial leather, but these methods often cannot guarantee the high gloss, high transparency and high-quality touch of the product at the same time, and are prone to defects such as pinholes and bubbles. Summary of the invention
[0003] In order to solve at least one of the above technical problems, a method for preparing a dual-process mirror high-transmittance crystal leather is developed.
[0004] On the one hand, the present application provides a method for preparing a dual-process mirror high-transmittance crystal leather, comprising the following steps: Process 1: Preparation of semi-finished leather products, including the following steps: A1. Evenly apply a layer of pearlescent surface polyurethane slurry with a thickness of 10-13 filaments on the textured release paper, and then dry the surface layer at a temperature of 90-120°C to obtain a pearlescent surface polyurethane film, wherein the viscosity of the pearlescent surface polyurethane slurry is 3000-6000 cps / 25°C; A2. Evenly apply a layer of colored middle layer polyurethane slurry with a thickness of 15-22 filaments on the pearlescent surface layer, and then dry the surface layer at 80-120°C to obtain a colored polyurethane middle layer, wherein the viscosity of the colored middle layer polyurethane slurry is 5000-10000 cps / 20°C, and then evenly apply a layer of adhesive layer polyurethane slurry with a thickness of 15-25 filaments on the colored middle layer film, and bake the adhesive layer at 50-60°C to a semi-dry and wet state, and then use a laminating roller to bond it with a weft-knitted stretch knitted fabric, and then dry it at 125-145°C and cool it, and peel off the release paper to obtain a semi-finished pearlescent texture polyurethane leather, wherein the viscosity of the adhesive layer polyurethane slurry is 30000-50000 cps / 25°C; Second process: mirror release paper transfer lamination, including the following steps: B1. Evenly coating a layer of high modulus surface polyurethane colorless slurry with a thickness of 13-18 filaments on the mirror release paper, and drying the surface polyurethane colorless slurry at a temperature of 90-110° C. to obtain a transparent surface polyurethane film, wherein the viscosity of the surface polyurethane colorless slurry is 3000-5000 cps / 25° C.; B2. A layer of polyurethane colorless adhesive layer slurry with a thickness of 20-35 filaments is evenly coated on the transparent surface polyurethane film, and dried at 90-120°C for 1-2 minutes to evaporate part of the polyurethane colorless slurry solvent and make the polyurethane colorless adhesive slurry film in a semi-dry state, and add appropriate amount of clean water. At the same time, a laminating roller is used to bond the pearlescent texture polyurethane leather semi-finished product, and the viscosity of the adhesive layer polyurethane colorless slurry is 15000-25000 cps / 25°C; then put it into an oven at a temperature of 135-150°C for 4-6 minutes, and finally cool it and peel off the mirror release paper to obtain the double-process mirror high-transparency crystal leather finished product.
[0005] Optionally, in the process, the pearlescent surface layer polyurethane slurry is made of the following components in parts by weight: 100 parts of polyurethane resin, 8-20 parts of dimethylformamide, 20-50 parts of dimethyl carbonate, and 1-5 parts of pearl powder.
[0006] Optionally, in the process, the colored middle layer polyurethane slurry is made of the following components in parts by weight: 100 parts of polyurethane resin, 8-20 parts of dimethylformamide, 20-50 parts of dimethyl carbonate, and 5-15 parts of colorant.
[0007] Optionally, in the process, the adhesive layer polyurethane slurry is made of the following components in parts by weight: 100 parts of polyurethane resin, 5-20 parts of dimethylformamide, and 5-20 parts of dimethyl carbonate.
[0008] Optionally, in step A2, the thickness of the weft-knitted stretch fabric is 0.4-0.5 mm.
[0009] Optionally, in the second process, the high modulus surface layer polyurethane colorless slurry is made of the following components in parts by weight: 100 parts of polyurethane resin and 40-80 parts of dimethylformamide.
[0010] Optionally, in the second process, the adhesive layer polyurethane slurry is made of the following components in parts by weight: 100 parts of polyurethane resin, 5-20 parts of dimethylformamide, and 5-20 parts of dimethyl carbonate.
[0011] Optionally, in step A2, the gap between the pressure rollers is 0.3-0.8 mm.
[0012] Optionally, in step B2, the gap between the pressure rollers is 0.2-0.6 mm.
[0013] The present invention includes at least one of the following beneficial technical effects: 1. This application uses a dual-process technology, combining dry lamination and semi-dry lamination technology, so that the high-transparency crystal leather finally produced has significant crystal luster, high transparency, three-dimensional texture without pinholes and bubbles, bright colors and smooth surface touch, meeting the stringent requirements of the high-end market for artificial leather. At the same time, it has excellent wear resistance and folding resistance.
[0014] 2. The preparation method of the present application has strong production operability and is suitable for industrial promotion. DETAILED DESCRIPTION
[0015] The present application is further described in detail below with reference to the embodiments.
[0016] The present application designs a method for preparing a double-process mirror-like high-transmittance crystal leather, comprising the following steps: Specific embodiments Example 1 A method for preparing a double-process mirror-surface high-transmittance crystal leather comprises the following steps: Process 1: Preparation of semi-finished leather products, including the following steps: A1. 100 parts of polyurethane resin, 14 parts of dimethylformamide, 35 parts of dimethyl carbonate and 3 parts of pearl powder were mixed and stirred to obtain a pearl surface polyurethane slurry with a viscosity of 4500 cps / 25°C. A layer of the pearl surface polyurethane slurry with a thickness of 12 threads was evenly coated on the textured release paper, and then the surface layer was dried at 110°C to obtain a pearl surface polyurethane film; A2. 100 parts of polyurethane resin, 15 parts of dimethylformamide, 30 parts of dimethyl carbonate and 10 parts of colorant were mixed and stirred evenly to obtain a colored middle layer polyurethane slurry with a viscosity of 7000 cps / 20°C. A layer of colored middle layer polyurethane slurry with a thickness of 18 threads was evenly applied on the pearlescent surface layer, and then the surface layer was dried at a temperature of 100°C to obtain a colored polyurethane middle layer; 100 parts of polyurethane resin, 13 parts of dimethylformamide and 13 parts of dimethyl carbonate were mixed and stirred evenly to obtain a colored middle layer polyurethane slurry with a viscosity of 40000 cps / 20°C. cps / 20℃ adhesive layer polyurethane slurry, and then evenly scrape a layer of 20-filament adhesive layer polyurethane slurry on the colored middle layer film, bake the adhesive layer at 55℃ to a semi-dry and wet state, and then use a laminating roller to bond it with the weft-knitted stretch knitted fabric, and then dry it at 135℃ and cool it, and peel off the release paper to obtain a pearlescent texture polyurethane leather semi-finished product; wherein, the gap between the pressure rollers is 0.5mm, and the thickness of the weft-knitted stretch knitted fabric is 0.4mm.
[0017] Second process: mirror release paper transfer lamination, including the following steps: B1. 100 parts of polyurethane resin and 60 parts of dimethylformamide were mixed and stirred to obtain a high modulus surface polyurethane colorless slurry with a viscosity of 4000cps / 25°C. A layer of high modulus surface polyurethane colorless slurry with a thickness of 15 filaments was evenly coated on the mirror release paper, and the surface polyurethane colorless slurry was dried at 100°C to obtain a transparent surface polyurethane film. B2. 100 parts of polyurethane resin, 12 parts of dimethylformamide and 12 parts of dimethyl carbonate are mixed and stirred evenly to obtain a bonding layer polyurethane colorless slurry with a viscosity of 20,000 cps / 25°C, and a layer of bonding layer polyurethane colorless slurry with a thickness of 28 threads is evenly coated on the transparent surface polyurethane film, and dried at 110°C for 2 minutes to evaporate part of the solvent of the bonding layer polyurethane colorless slurry and make the bonding layer polyurethane colorless adhesive slurry film in a semi-dry state, and add appropriate amount of clean water. At the same time, the pearlescent texture polyurethane leather semi-finished product is laminated with a laminating roller, and then put into an oven at a temperature of 142°C for drying for 5 minutes, and finally cooled and the mirror release paper is peeled off to obtain the double-process mirror high-transparency crystal leather finished product; wherein, the gap between the pressing rollers is 0.4mm.
[0018] Example 2 A method for preparing a double-process mirror-surface high-transmittance crystal leather comprises the following steps: Process 1: Preparation of semi-finished leather products, including the following steps: A1. 100 parts of polyurethane resin, 20 parts of dimethylformamide, 50 parts of dimethyl carbonate and 5 parts of pearl powder were mixed and stirred to obtain a pearl surface polyurethane slurry with a viscosity of 3000 cps / 25°C. A layer of the pearl surface polyurethane slurry with a thickness of 13 threads was evenly coated on the textured release paper, and then the surface layer was dried at 120°C to obtain a pearl surface polyurethane film; A2. 100 parts of polyurethane resin, 20 parts of dimethylformamide, 50 parts of dimethyl carbonate and 15 parts of colorant were mixed and stirred evenly to obtain a colored middle layer polyurethane slurry with a viscosity of 5000 cps / 20°C. A layer of colored middle layer polyurethane slurry with a thickness of 22 filaments was evenly applied on the pearlescent surface layer, and then the surface layer was dried at a temperature of 120°C to obtain a colored polyurethane middle layer; 100 parts of polyurethane resin, 20 parts of dimethylformamide and 20 parts of dimethyl carbonate were mixed and stirred evenly to obtain a colored middle layer polyurethane slurry with a viscosity of 30000 cps / 20°C. cps / 20℃ adhesive layer polyurethane slurry, and then evenly scrape a layer of 25-filament adhesive layer polyurethane slurry on the colored middle layer film, bake the adhesive layer at 60℃ to a semi-dry and wet state, and then use a laminating roller to bond it with the weft-knitted stretch knitted fabric, and then dry it at 145℃ and cool it, and peel off the release paper to obtain a pearlescent texture polyurethane leather semi-finished product; wherein, the gap between the pressing rollers is 0.3mm, and the thickness of the weft-knitted stretch knitted fabric is 0.5mm.
[0019] Second process: mirror release paper transfer lamination, including the following steps: B1. 100 parts of polyurethane resin and 80 parts of dimethylformamide were mixed and stirred to obtain a high modulus surface polyurethane colorless slurry with a viscosity of 3000cps / 25°C. A layer of high modulus surface polyurethane colorless slurry with a thickness of 18 filaments was evenly coated on the mirror release paper, and the surface polyurethane colorless slurry was dried at a temperature of 110°C to obtain a transparent surface polyurethane film. B2. 100 parts of polyurethane resin, 20 parts of dimethylformamide and 20 parts of dimethyl carbonate are mixed and stirred evenly to obtain a bonding layer polyurethane colorless slurry with a viscosity of 15000 cps / 25°C, and a layer of bonding layer polyurethane colorless slurry with a thickness of 35 silk is evenly coated on the transparent surface polyurethane film, and dried at 120°C for 2 minutes to evaporate part of the solvent of the bonding layer polyurethane colorless slurry and make the bonding layer polyurethane colorless adhesive slurry film in a semi-dry state, and add appropriate amount of clean water. At the same time, the pearlescent texture polyurethane leather semi-finished product is laminated with a laminating roller, and then put into an oven at a temperature of 150°C for drying for 6 minutes, and finally cooled and the mirror release paper is peeled off to obtain the double-process mirror high-transparency crystal leather finished product; wherein, the gap between the pressing rollers is 0.2mm.
[0020] Example 3 A method for preparing a double-process mirror-surface high-transmittance crystal leather comprises the following steps: Process 1: Preparation of semi-finished leather products, including the following steps: A1. 100 parts of polyurethane resin, 8 parts of dimethylformamide, 20 parts of dimethyl carbonate and 1 part of pearl powder were mixed and stirred to obtain a pearl surface polyurethane slurry with a viscosity of 6000 cps / 25°C. A layer of the pearl surface polyurethane slurry with a thickness of 10 filaments was evenly coated on the textured release paper, and then the surface layer was dried at 90°C to obtain a pearl surface polyurethane film; A2, 100 parts of polyurethane resin, 8 parts of dimethylformamide, 20 parts of dimethyl carbonate and 5 parts of colorant were mixed and stirred to obtain a viscosity of 10000 cps / 20℃ colored middle layer polyurethane slurry, evenly apply a layer of colored middle layer polyurethane slurry with a thickness of 15 silks on the pearlescent surface layer, and then dry the surface layer at 80℃ to obtain a colored polyurethane middle layer; 100 parts of polyurethane resin, 5 parts of dimethylformamide and 5 parts of dimethyl carbonate are mixed and stirred evenly to obtain an adhesive layer polyurethane slurry with a viscosity of 50000cps / 20℃, and then evenly apply a layer of adhesive layer polyurethane slurry with a thickness of 25 silks on the colored middle layer film, bake the adhesive layer at 50℃ to a semi-dry and wet state, and then use a laminating roller to bond it with a weft-knitted stretch knitted fabric, and then dry it at 125℃ and cool it, and peel off the release paper to obtain a pearlescent texture polyurethane leather semi-finished product; wherein, the gap between the rollers is 0.8mm, and the thickness of the weft-knitted stretch knitted fabric is 0.4mm.
[0021] Second process: mirror release paper transfer lamination, including the following steps: B1. 100 parts of polyurethane resin and 40 parts of dimethylformamide were mixed and stirred to obtain a high modulus surface polyurethane colorless slurry with a viscosity of 5000cps / 25°C. A layer of high modulus surface polyurethane colorless slurry with a thickness of 13 filaments was evenly coated on the mirror release paper, and the surface polyurethane colorless slurry was dried at 90°C to obtain a transparent surface polyurethane film. B2. 100 parts of polyurethane resin, 5 parts of dimethylformamide and 5 parts of dimethyl carbonate are mixed and stirred evenly to obtain a bonding layer polyurethane colorless slurry with a viscosity of 25000 cps / 25°C, and a layer of bonding layer polyurethane colorless slurry with a thickness of 20 silk is evenly coated on the transparent surface polyurethane film, and dried at 90°C for 1 minute to evaporate part of the solvent of the bonding layer polyurethane colorless slurry and make the bonding layer polyurethane colorless adhesive slurry film in a semi-dry state, and add appropriate amount of clean water. At the same time, the pearlescent texture polyurethane leather semi-finished product is laminated with a laminating roller, and then put into an oven at a temperature of 135°C for drying for 4 minutes, and finally cooled and the mirror release paper is peeled off to obtain the double-process mirror high-transparency crystal leather finished product; wherein, the gap between the pressing rollers is 0.6mm.
[0022] Comparative Example 1 A method for preparing a double-process mirror-surface high-transmittance crystal leather comprises the following steps: Process 1: Preparation of semi-finished leather products, including the following steps: A1. 100 parts of polyurethane resin, 20 parts of dimethylformamide, 50 parts of dimethyl carbonate and 5 parts of pearl powder were mixed and stirred to obtain a pearl surface polyurethane slurry with a viscosity of 3000 cps / 25°C. A layer of the pearl surface polyurethane slurry with a thickness of 13 threads was evenly coated on the textured release paper, and then the surface layer was dried at 120°C to obtain a pearl surface polyurethane film; A2. 100 parts of polyurethane resin, 20 parts of dimethylformamide, 50 parts of dimethyl carbonate and 15 parts of colorant were mixed and stirred to obtain a colored middle layer polyurethane slurry with a viscosity of 5000 cps / 20°C, and a layer of colored middle layer polyurethane slurry with a thickness of 22 filaments was evenly applied on the pearlescent surface layer, and then the surface layer was dried at a temperature of 120°C to obtain a colored polyurethane middle layer; 100 parts of polyurethane resin, 20 parts of dimethylformamide and 20 parts of dimethyl carbonate were mixed and stirred to obtain an adhesive layer polyurethane slurry with a viscosity of 30000 cps / 20°C, and then a layer of adhesive layer polyurethane slurry with a thickness of 25 filaments was evenly applied on the colored middle layer film, the adhesive layer was dried at a temperature of 145°C, and then laminated with a weft-knitted stretch knitted fabric using a laminating roller, and the release paper was peeled off to obtain a semi-finished pearlescent texture polyurethane leather; wherein, the gap between the rollers was 0.3mm, and the thickness of the weft-knitted stretch knitted fabric was 0.5mm.
[0023] Second process: mirror release paper transfer lamination, including the following steps: B1. 100 parts of polyurethane resin and 80 parts of dimethylformamide were mixed and stirred to obtain a high modulus surface polyurethane colorless slurry with a viscosity of 3000cps / 25°C. A layer of high modulus surface polyurethane colorless slurry with a thickness of 18 filaments was evenly coated on the mirror release paper, and the surface polyurethane colorless slurry was dried at a temperature of 110°C to obtain a transparent surface polyurethane film. B2. 100 parts of polyurethane resin, 20 parts of dimethylformamide and 20 parts of dimethyl carbonate are mixed and stirred evenly to obtain a colorless adhesive layer polyurethane slurry with a viscosity of 15000 cps / 25°C, and a layer of colorless adhesive layer polyurethane slurry with a thickness of 35 filaments is evenly coated on the transparent surface polyurethane film. After drying at 120°C, the semi-finished pearlescent polyurethane leather is laminated with a laminating roller. Finally, the semi-finished product is cooled and the mirror release paper is peeled off to obtain the double-process mirror high-transparency crystal leather finished product; wherein the gap between the rollers is 0.2 mm.
[0024] Effect test 1. Observe and touch the mirror-like high-transmittance crystal leather prepared in Examples 1-3 and Comparative Example 1.
[0025] 2. The mirror-like high-transmittance crystal leathers prepared in Examples 1-3 and Comparative Example 1 were subjected to Martindale test and surface folding resistance test in turn.
[0026] Test Results 1. The mirror-like high-transparency crystal leather prepared in Examples 1-3 has significant crystal luster, high transparency, three-dimensional texture, no pinholes, bubbles, bright colors and smooth surface touch. The mirror-like high-transparency crystal leather prepared in Comparative Example 1 has a slightly darker luster and has defects such as pinholes and bubbles.
[0027] 2. The mirror-like high-transmittance crystal leather prepared in Examples 1-3 had no cracks on the leather surface when tested 50,000 times by Martindale; and had no cracks on the leather surface when folded 100,000 times at room temperature (about 25°C). However, the mirror-like high-transmittance crystal leather prepared in Comparative Example 1 cracked. Therefore, the mirror-like high-transmittance crystal leather prepared in this application has excellent surface wear resistance and folding resistance.
[0028] This application uses a dual-process technology, combining dry lamination and semi-dry lamination technology, so that the final mirror-like high-transparency crystal leather has a significant crystal luster, high transparency, three-dimensional texture, and no pinholes or bubbles. At the same time, the color is bright and the surface is smooth to the touch, meeting the stringent requirements of the high-end market for artificial leather.
[0029] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing a double-process mirror high-transmittance crystal leather, It is characterized in that The steps include: Process 1: Preparation of semi-finished leather products, including the following steps: A1. Evenly apply a layer of pearlescent surface polyurethane slurry with a thickness of 10-13 filaments on the textured release paper, and then dry the surface layer at a temperature of 90-120°C to obtain a pearlescent surface polyurethane film, wherein the viscosity of the pearlescent surface polyurethane slurry is 3000-6000 cps / 25°C; A2. Evenly apply a layer of colored middle layer polyurethane slurry with a thickness of 15-22 filaments on the pearlescent surface layer, and then dry the surface layer at 80-120°C to obtain a colored polyurethane middle layer, wherein the viscosity of the colored middle layer polyurethane slurry is 5000-10000 cps / 20°C, and then evenly apply a layer of adhesive layer polyurethane slurry with a thickness of 15-25 filaments on the colored middle layer film, and bake the adhesive layer at 50-60°C to a semi-dry and wet state, and then use a laminating roller to bond it with a weft-knitted stretch knitted fabric, and then dry it at 125-145°C and cool it, and peel off the release paper to obtain a semi-finished pearlescent texture polyurethane leather, wherein the viscosity of the adhesive layer polyurethane slurry is 30000-50000 cps / 25°C; Second process: mirror release paper transfer lamination, including the following steps: B1. Evenly coating a layer of high modulus surface polyurethane colorless slurry with a thickness of 13-18 filaments on the mirror release paper, and drying the surface polyurethane colorless slurry at a temperature of 90-110° C. to obtain a transparent surface polyurethane film, wherein the viscosity of the surface polyurethane colorless slurry is 3000-5000 cps / 25° C.; B2. A layer of polyurethane colorless adhesive layer slurry with a thickness of 20-35 filaments is evenly coated on the transparent surface polyurethane film, and dried at 90-120°C for 1-2 minutes to evaporate part of the polyurethane colorless slurry solvent and make the polyurethane colorless adhesive slurry film in a semi-dry state, and add appropriate amount of clean water. At the same time, a laminating roller is used to bond the pearlescent texture polyurethane leather semi-finished product, and the viscosity of the adhesive layer polyurethane colorless slurry is 15000-25000 cps / 25°C; then put it into an oven at a temperature of 135-150°C for 4-6 minutes, and finally cool it and peel off the mirror release paper to obtain the double-process mirror high-transparency crystal leather finished product.
2. The method for preparing the double-process mirror high-transmittance crystal leather according to claim 1, It is characterized in that In the process, the pearlescent surface layer polyurethane slurry is made of the following components in parts by weight: 100 parts of polyurethane resin, 8-20 parts of dimethylformamide, 20-50 parts of dimethyl carbonate, and 1-5 parts of pearl powder.
3. The method for preparing the double-process mirror high-transmittance crystal leather according to claim 1, It is characterized in that In the process, the colored middle layer polyurethane slurry is made of the following components in parts by weight: 100 parts of polyurethane resin, 8-20 parts of dimethylformamide, 20-50 parts of dimethyl carbonate, and 5-15 parts of colorant.
4. The method for preparing the double-process mirror high-transmittance crystal leather according to claim 1, It is characterized in that In the process, the adhesive layer polyurethane slurry is made of the following components in parts by weight: 100 parts of polyurethane resin, 5-20 parts of dimethylformamide, and 5-20 parts of dimethyl carbonate.
5. The method for preparing the double-process mirror high-transmittance crystal leather according to claim 1, It is characterized in that In the step A2, the thickness of the weft-knitted stretch knitted fabric is 0.4-0.5 mm.
6. The method for preparing the double-process mirror high-transmittance crystal leather according to claim 1, It is characterized in that In the second process, the high modulus surface layer polyurethane colorless slurry is made of the following components in parts by weight: 100 parts of polyurethane resin and 40-80 parts of dimethylformamide.
7. The method for preparing the double-process mirror high-transmittance crystal leather according to claim 1, It is characterized in that In the second process, the adhesive layer polyurethane slurry is made of the following components in parts by weight: 100 parts of polyurethane resin, 5-20 parts of dimethylformamide, and 5-20 parts of dimethyl carbonate.
8. The method for preparing the double-process mirror high-transmittance crystal leather according to claim 1, It is characterized in that In step A2, the gap between the pressing rollers is 0.3-0.8 mm.
9. The method for preparing the double-process mirror high-transmittance crystal leather according to claim 1, It is characterized in that In step B2, the gap between the pressing rollers is 0.2-0.6 mm.