High-barrier food packaging paper and production process thereof
Patent Information
- Application Number
- CN202410977509.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-22
AI Technical Summary
The barrier properties of existing food packaging paper are of high cost and poor promotion, especially the large amount of oil-proofing agent and high cost, making it difficult to meet the needs of efficient waterproofing and oil-proofing.
After mixing and reacting with plant fibers and alkali liquid, filtering, washing, and mechanical slurrying is carried out. The secondary fiber slurry is generated by high-pressure homogenization treatment, and mixed with sodium alginate sol, alkyd resin, and talc powder to form a mixed slurry. After crafting, and glue-adding treatment to prepare high-barrier food packaging paper.
It reduces production costs, improves the barrier properties, tensile strength and breakage resistance of packaging paper, and at the same time enhances the uniformity of fiber dispersion, and improves the overall structure and oil resistance of packaging paper.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to high-barrier food packaging paper and a production process thereof, and belongs to the field of papermaking. Background Art
[0002] Food wrapping paper is a paper packaging material for candies, popsicles, cakes and other foods that are eaten directly. Food wrapping paper plays an irreplaceable role in protecting food, preventing food from being contaminated by external microorganisms or other substances, and preventing or reducing food oxidation and other reactions. Therefore, wrapping paper must have good barrier properties (waterproof and oilproof).
[0003] In order to make the packaging paper have high barrier properties, it is usually necessary to apply sizing to the surface of the paper, and add an oil-proofing agent to the surface sizing agent to improve the oil-proofing effect. Many oil-proofing agents developed with natural polymers as raw materials or fluorine-free oil-proofing agents have been developed accordingly, and are also applied to the surface of paper by sizing. However, this type of oil-proofing agent has the problem of large dosage and high cost, and its promotion is poor. Summary of the invention
[0004] The purpose of the present invention is to provide a high barrier food packaging paper and a production process thereof, so as to solve the problem of how to improve the barrier properties of the packaging paper while reducing the cost. To this end, the present invention provides a production process for high barrier food packaging paper, comprising the following steps:
[0005] a) mixing plant fiber with alkali solution for reaction, filtering, washing, drying in sequence, adding water and mechanically beating to obtain primary fiber slurry;
[0006] b) subjecting the primary fiber slurry to shearing treatment for 5-10 minutes and then transferring it to a high-pressure homogenizer for homogenization to obtain a secondary fiber slurry;
[0007] c) stirring the secondary fiber slurry, sodium alginate sol, alkyd resin and talcum powder at 30-40° C. for 0.5-1 h to obtain a mixed slurry;
[0008] d) sequentially papermaking and drying the mixed slurry to obtain base paper;
[0009] e) sizing and drying the base paper to obtain high-barrier food packaging paper.
[0010] In the preferred technical scheme of the above production process, the preparation method of the sodium alginate sol includes adding tea polyphenols and sodium alginate to an acetic acid solution, stirring evenly, adjusting the pH value to 4-6 with an alkaline solution, and continuing to stir at 30-50°C for 20-60 minutes to obtain the sodium alginate sol.
[0011] In the preferred technical scheme of the above production process, the mass ratio of the tea polyphenols, sodium alginate and acetic acid solution is (0.3-1):(1-5):100, and the mass concentration of the acetic acid solution is 0.5-1.5%.
[0012] In the preferred technical solution of the above production process, the homogenization process specifically includes:
[0013] At a pressure of 40-50Mpa, cycle 2-4 times;
[0014] Under the pressure of 20-30Mpa, cycle 1-3 times;
[0015] At a pressure of 30-40Mpa, cycle 1-3 times.
[0016] In the preferred technical scheme of the above production process, the preparation method of the sizing agent used for sizing includes:
[0017] Add solvent to alkyd resin, octenyl succinic anhydride and lauryl amide propyl betaine, stir evenly, add modified cellulose and modified cyclodextrin in sequence, react at 50-70°C for 10-15h, then add silane coupling agent, stir at 40-50°C for 2-4h to obtain a sizing agent.
[0018] In the preferred technical scheme of the above production process, the mass ratio of alkyd resin, octenylsuccinic anhydride, lauryl amide propyl betaine, silane coupling agent, modified cellulose and modified cyclodextrin is (1-3): (0.5-1): (0.3-0.6): (0.05-0.1): (0.1-0.5): (0.1-0.5).
[0019] In the preferred technical scheme of the above production process, the preparation method of modified cellulose and modified cyclodextrin includes:
[0020] The cellulose suspension and the cyclodextrin suspension are mixed and then subjected to ultrasonic treatment, stearic acid and sodium alginate are then added and ultrasonic treatment is continued, and then stirred for 10-15 hours in a water bath, and modified cellulose and modified cyclodextrin are obtained after centrifugation and drying.
[0021] In the preferred technical scheme of the above production process, the mass ratio of secondary fiber slurry, sodium alginate sol, alkyd resin and talcum powder is 100:(10-20):(1-5):(1-5).
[0022] In the preferred technical solution of the above production process, the beating degree of the primary fiber slurry is 60-70°SR; and / or
[0023] The mass concentration of the primary fiber slurry is 10-15%.
[0024] The present invention also provides a high-barrier food packaging paper produced by the production process described in the above preferred technical solution.
[0025] Another object of the present invention is to provide a high barrier food packaging paper and a production process thereof, wherein the fiber size can be reduced, the fiber dispersion uniformity can be improved, the internal structure of the packaging paper can be enhanced, and the barrier performance of the packaging paper can be improved by homogenizing the primary fiber slurry. In addition, the secondary fiber slurry, sodium alginate sol, alkyd resin, and talcum powder are used as raw materials to reduce the production cost, improve the barrier performance of the food packaging paper, and improve the oil resistance of the packaging paper, while also improving the tensile strength and bursting strength of the packaging paper. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention can also be implemented in other ways different from those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0027] The present invention provides a production process for high-barrier food packaging paper, which is characterized by comprising the following steps:
[0028] a) mixing plant fiber with alkali solution for reaction, filtering, washing, drying in sequence, adding water and mechanically beating to obtain primary fiber slurry;
[0029] b) subjecting the primary fiber slurry to shearing treatment for 5-10 minutes and then transferring it to a high-pressure homogenizer for homogenization to obtain a secondary fiber slurry;
[0030] c) stirring the secondary fiber slurry, sodium alginate sol, alkyd resin and talcum powder at 30-40° C. for 0.5-1 h to obtain a mixed slurry;
[0031] d) sequentially papermaking and drying the mixed slurry to obtain base paper;
[0032] e) sizing and drying the base paper to obtain high-barrier food packaging paper.
[0033] The present application can reduce the fiber size, improve the fiber dispersion uniformity, strengthen the internal structure of the packaging paper, and improve the barrier performance of the packaging paper by homogenizing the primary fiber slurry. In addition, the secondary fiber slurry, sodium alginate sol, alkyd resin, and talcum powder are used as raw materials to reduce the production cost, improve the barrier performance of the food packaging paper, improve the oil resistance of the packaging paper, and at the same time improve the tensile strength and bursting strength of the packaging paper.
[0034] In step a), the present invention can destroy the lignin structure by subjecting the plant fiber to alkali treatment, and then separate the lignin from the fiber by filtering and washing. The mass concentration of the primary fiber slurry obtained by mechanical beating is 10-15%, and the beating degree is 60-70°SR. The primary fiber slurry with this beating degree can improve the barrier performance of the device.
[0035] The plant fibers include wood fibers and bamboo fibers, wherein the weight ratio of the wood fibers to the bamboo fibers is (1-9): (9-1).
[0036] In step b), the primary fiber slurry is subjected to high-quality treatment, wherein the high-quality treatment step includes treating at a pressure of 40-50Mpa for 5-10 minutes; treating at a pressure of 20-30Mpa for 3-6 minutes; and treating at a pressure of 30-40Mpa for 3-6 minutes. By subjecting the primary fiber slurry to high-quality treatment, nanocellulose fibrils can be obtained, thereby improving the barrier properties of the packaging paper.
[0037] In step c), using secondary fiber slurry, sodium alginate sol, alkyd resin and talcum powder as raw materials for packaging paper can improve the oil resistance, tensile strength and bursting strength of the packaging paper. The mass ratio of secondary fiber slurry, sodium alginate sol, alkyd resin and talcum powder is 100:(10-20):(1-5):(1-5).
[0038] Sodium alginate sol can improve the antibacterial and anticorrosive properties of food packaging paper. The preparation method of sodium alginate sol is as follows: tea polyphenols and sodium alginate are added to acetic acid solution, stirred evenly, pH value is adjusted to 4-6 with alkaline solution, and then stirred at 30-50°C for 20-60 minutes to obtain sodium alginate sol. The mass ratio of tea polyphenols, sodium alginate and acetic acid solution is (0.3-1): (1-5): 100, and the mass concentration of acetic acid solution is 0.5-1.5%.
[0039] Talc can improve the tear resistance of packaging paper, and its particle size is 100-200nm.
[0040] Alkyd resins can improve the tensile strength and bursting strength of packaging paper.
[0041] The steps d) of papermaking and drying are conventional techniques in the art and will not be described in detail here.
[0042] In step e), sizing is performed on the surface of the base paper, which can improve the barrier properties of the packaging paper on the one hand, and can improve the tensile strength and bursting strength of the packaging paper on the other hand.
[0043] The preparation method of the sizing agent used for sizing comprises:
[0044] Add solvent to alkyd resin, octenyl succinic anhydride and lauryl amide propyl betaine, stir evenly, add modified cellulose and modified cyclodextrin in sequence, react at 50-70°C for 10-15h, then add silane coupling agent, stir at 40-50°C for 2-4h to obtain a sizing agent.
[0045] The mass ratio of alkyd resin, octenyl succinic anhydride, lauryl amide propyl betaine, silane coupling agent, modified cellulose and modified cyclodextrin is (1-3): (0.5-1): (0.3-0.6):
[0046] (0.05-0.1):(0.1-0.5):(0.1-0.5).
[0047] By using alkyd resin in the sizing agent, the peel strength between the sizing layer and the base paper can be improved, and the carboxyl groups in octenyl succinic anhydride and lauryl amide propyl betaine can react with the hydroxyl groups in the alkyd resin to improve the film-forming effect of the sizing agent, thereby improving the barrier properties of the sizing layer.
[0048] In the above steps, the solvent may be any one of tetrahydrofuran, N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.
[0049] The silane coupling agent is any one of ethyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane and propyltriethoxysilane.
[0050] Wherein, the preparation method of modified cellulose and modified cyclodextrin comprises:
[0051] The cellulose suspension and the cyclodextrin suspension are mixed and then ultrasonically treated, stearic acid and sodium alginate are added and ultrasonicated, and then stirred for 10-15 hours in a water bath, centrifuged and dried to obtain modified cellulose and modified cyclodextrin. The mass concentration of the cellulose suspension is 1-3%, and the mass concentration of the cyclodextrin suspension is 1-3%. The mass ratio of the cellulose suspension, the cyclodextrin suspension, stearic acid and sodium alginate is (10-90): (10-90): (1-2): (1-5). By modifying cellulose and cyclodextrin, the film-forming performance of the sizing agent can be improved, thereby ensuring the barrier performance of the packaging paper.
[0052] The present invention is illustrated with reference to the following examples.
[0053] The sodium alginate, alkyd resin, talc, tea polyphenols, octenyl succinic anhydride, lauramide propyl betaine, cellulose, cyclodextrin, silane coupling agent, and solvent used in the present application are all commercially available.
[0054] The silane coupling agent is ethyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane or propyltriethoxysilane, all of which are purchased from TCI (Shanghai) Chemical Industry Development Co., Ltd.
[0055] The solvents were tetrahydrofuran, N,N-dimethylformamide, N,N-dimethylacetamide or dimethyl sulfoxide, all purchased from Jinan Chuangshi Chemical Co., Ltd.
[0056] Sodium alginate was purchased from Shandong Jingyun Food Ingredients Co., Ltd.
[0057] Alkyd resin was purchased from Shandong Lingsai Paint Co., Ltd., 389-9A.
[0058] Talc was purchased from Danhai Chemical Stone Powder Co., Ltd. in Haicheng City.
[0059] Tea polyphenols were purchased from Xi'an Best Biotechnology Co., Ltd.
[0060] Octenyl succinic anhydride was purchased from Guangzhou Chuancan Chemical Co., Ltd.
[0061] Lauryl amide propyl betaine was purchased from Shengci (Hubei) Industrial Materials Co., Ltd.
[0062] Cellulose is microcrystalline cellulose or carboxymethyl cellulose, both purchased from Guangzhou Huayu Biotechnology Co., Ltd.
[0063] Cyclodextrin was α-cyclodextrin purchased from Shanghai Baisifu Food Development Co., Ltd.
[0064] In addition, wood fiber and bamboo fiber are obtained by the following method: processing wood raw materials or bamboo raw materials into small shapes, then steaming the materials, and then hot grinding, drying, and sieving to obtain wood fiber powder or bamboo fiber powder, and then controlling the moisture content of the wood fiber powder or bamboo fiber powder to 40-50% (mass percentage), and finally using laccase or white rot fungi to treat the wood fiber powder or bamboo fiber powder to obtain wood fiber powder or bamboo fiber powder.
[0065] Example 1
[0066] The production process of high barrier food packaging paper includes the following steps:
[0067] a) mixing plant fiber with alkali solution for reaction, filtering, washing, drying in sequence, adding water and mechanically beating to obtain a primary fiber pulp with a mass concentration of 11% and a beating degree of 60°SR;
[0068] The plant fiber includes wood fiber and bamboo fiber in a mass ratio of 1:1, and the alkali solution is a sodium hydroxide solution with a mass concentration of 2%;
[0069] b) subjecting the primary fiber slurry to shearing treatment for 7 minutes and then transferring it to a high-pressure homogenizer for homogenization to obtain a secondary fiber slurry;
[0070] The homogenization treatment includes: 3 cycles at a pressure of 45 MPa; 2 cycles at a pressure of 25 MPa; 2 cycles at a pressure of 35 MPa;
[0071] c) stirring the secondary fiber slurry, sodium alginate sol, alkyd resin and talc at 40° C. for 0.5 h to obtain a mixed slurry;
[0072] The mass ratio of secondary fiber slurry, sodium alginate sol, alkyd resin and talcum powder is 100:18:2:4;
[0073] The preparation method of sodium alginate sol is as follows: adding tea polyphenols and sodium alginate to acetic acid solution, stirring evenly, adjusting the pH value to 5 with an alkaline solution, and continuing to stir at 40°C for 40 minutes to obtain sodium alginate sol. The mass ratio of tea polyphenols, sodium alginate and acetic acid solution is 0.4:2:100, the mass concentration of acetic acid solution is 1.2%; and the particle size of talc powder is 100-200nm.
[0074] d) sequentially papermaking and drying the mixed slurry to obtain base paper;
[0075] e) sizing and drying the base paper to obtain high-barrier food packaging paper;
[0076] The preparation method of the sizing agent used for sizing comprises:
[0077] Tetrahydrofuran was added to alkyd resin, octenylsuccinic anhydride and lauramide propyl betaine, and the mixture was stirred evenly. Modified cellulose and modified cyclodextrin were added in sequence, and the mixture was reacted at 55°C for 13 hours. Ethyltrimethoxysilane was then added, and the mixture was stirred at 43°C for 3.5 hours to obtain a sizing agent. The mass ratio of alkyd resin, octenylsuccinic anhydride, lauramide propyl betaine, ethyltrimethoxysilane, modified cellulose and modified cyclodextrin was 2.5:0.9:0.55:0.09:0.25:0.35.
[0078] The preparation method of modified cellulose and modified cyclodextrin comprises:
[0079] The cellulose suspension and the cyclodextrin suspension were mixed and then ultrasonically treated. After 20 minutes, stearic acid and sodium alginate were added and ultrasonicated. The mixture was stirred for 30 minutes in a water bath at 45°C for 12 hours, and then centrifuged and dried to obtain modified cellulose and modified cyclodextrin. The mass concentration of the cellulose suspension was 1.5%, and the mass concentration of the cyclodextrin suspension was 2.5%. The mass ratio of the cellulose suspension, the cyclodextrin suspension, the stearic acid and the sodium alginate was 90:10:1.5:2.
[0080] Example 2
[0081] The production process of high barrier food packaging paper includes the following steps:
[0082] a) mixing plant fiber with alkali solution for reaction, filtering, washing, drying in sequence, adding water and mechanically beating to obtain a primary fiber pulp with a mass concentration of 13% and a beating degree of 65°SR;
[0083] The plant fiber includes wood fiber and bamboo fiber in a mass ratio of 1:1, and the alkali solution is a potassium hydroxide solution with a mass concentration of 4%;
[0084] b) subjecting the primary fiber slurry to shearing treatment for 10 minutes and then transferring it to a high-pressure homogenizer for homogenization to obtain a secondary fiber slurry;
[0085] The homogenization treatment includes: 3 cycles at a pressure of 50 MPa; 2 cycles at a pressure of 30 MPa; and 1 cycle at a pressure of 40 MPa.
[0086] c) stirring the secondary fiber slurry, sodium alginate sol, alkyd resin and talc at 35° C. for 1 hour to obtain a mixed slurry;
[0087] The mass ratio of secondary fiber slurry, sodium alginate sol, alkyd resin and talcum powder is 100:12:4:3;
[0088] The preparation method of sodium alginate sol is as follows: adding tea polyphenols and sodium alginate to acetic acid solution, stirring evenly, adjusting the pH value to 6 with an alkaline solution, and continuing to stir at 50°C for 45 minutes to obtain sodium alginate sol. The mass ratio of tea polyphenols, sodium alginate and acetic acid solution is 0.6:4:100, the mass concentration of acetic acid solution is 1.2%; and the particle size of talc powder is 100-200nm.
[0089] d) sequentially papermaking and drying the mixed slurry to obtain base paper;
[0090] e) sizing and drying the base paper to obtain high-barrier food packaging paper;
[0091] The preparation method of the sizing agent used in sizing includes:
[0092] N,N-dimethylformamide was added to alkyd resin, octenylsuccinic anhydride and laurylamidopropyl betaine, and the mixture was stirred evenly. Then modified cellulose and modified cyclodextrin were added in sequence, and the mixture was reacted at 55°C for 13 hours. Then methyltriethoxysilane was added, and the mixture was stirred at 40°C for 4 hours to obtain a sizing agent. The mass ratio of alkyd resin, octenylsuccinic anhydride, laurylamidopropyl betaine, methyltriethoxysilane, modified cellulose and modified cyclodextrin was 2.5:0.75:0.45:0.08:0.4:0.2.
[0093] The preparation method of modified cellulose and modified cyclodextrin comprises:
[0094] The cellulose suspension and the cyclodextrin suspension were mixed and then ultrasonically treated. After 10 minutes, stearic acid and sodium alginate were added and ultrasonicated. The mixture was stirred in a water bath at 50°C for 30 minutes and then stirred for 14 hours. The modified cellulose and modified cyclodextrin were obtained after centrifugation and drying. The mass concentration of the cellulose suspension was 1%, and the mass concentration of the cyclodextrin suspension was 1%. The mass ratio of the cellulose suspension, the cyclodextrin suspension, the stearic acid and the sodium alginate was 40:60:1.8:4.
[0095] Example 3
[0096] The production process of high barrier food packaging paper includes the following steps:
[0097] a) mixing plant fiber with alkali solution for reaction, filtering, washing, drying in sequence, adding water and mechanically beating to obtain a primary fiber pulp with a mass concentration of 12% and a beating degree of 65°SR;
[0098] The plant fiber includes wood fiber and bamboo fiber in a mass ratio of 1:1, and the alkali solution is a sodium hydroxide solution with a mass concentration of 2%;
[0099] b) subjecting the primary fiber slurry to shearing treatment for 5 minutes and then transferring it to a high-pressure homogenizer for homogenization to obtain a secondary fiber slurry;
[0100] The homogenization treatment includes: 3 cycles at a pressure of 40 MPa; 2 cycles at a pressure of 20 MPa; 2 cycles at a pressure of 30 MPa;
[0101] c) stirring the secondary fiber slurry, sodium alginate sol, alkyd resin and talc at 30° C. for 0.5 h to obtain a mixed slurry;
[0102] The mass ratio of secondary fiber slurry, sodium alginate sol, alkyd resin and talcum powder is 100:12:3:3;
[0103] The preparation method of sodium alginate sol is as follows: adding tea polyphenols and sodium alginate to acetic acid solution, stirring evenly, adjusting the pH value to 5 with an alkaline solution, and continuing to stir at 40°C for 30 minutes to obtain sodium alginate sol. The mass ratio of tea polyphenols, sodium alginate and acetic acid solution is 0.5:3:100, the mass concentration of acetic acid solution is 1%; and the particle size of talc powder is 100-200nm.
[0104] d) sequentially papermaking and drying the mixed slurry to obtain base paper;
[0105] e) sizing and drying the base paper to obtain high-barrier food packaging paper;
[0106] The preparation method of the sizing agent used for sizing comprises:
[0107] N,N-dimethylacetamide was added to alkyd resin, octenylsuccinic anhydride and laurylamidopropyl betaine, and the mixture was stirred evenly. Modified cellulose and modified cyclodextrin were added in sequence, and the mixture was reacted at 60°C for 12 hours. Ethyltriethoxysilane was then added, and the mixture was stirred at 45°C for 3 hours to obtain a sizing agent. The mass ratio of alkyd resin, octenylsuccinic anhydride, laurylamidopropyl betaine, ethyltriethoxysilane, modified cellulose and modified cyclodextrin was 2:0.7:0.4:0.08:0.3:0.3.
[0108] The preparation method of modified cellulose and modified cyclodextrin comprises:
[0109] The cellulose suspension and the cyclodextrin suspension were mixed and then ultrasonically treated. After 20 minutes, stearic acid and sodium alginate were added and ultrasonicated. After 20 minutes, the mixture was stirred in a water bath at 50°C for 10-15 hours, centrifuged and dried to obtain modified cellulose and modified cyclodextrin. The mass concentration of the cellulose suspension was 2%, and the mass concentration of the cyclodextrin suspension was 2%. The mass ratio of the cellulose suspension, the cyclodextrin suspension, the stearic acid and the sodium alginate was 50:50:1.5:3.
[0110] Example 4
[0111] The production process of high barrier food packaging paper includes the following steps:
[0112] a) mixing plant fiber with alkali solution for reaction, filtering, washing, drying in sequence, adding water and mechanically beating to obtain a primary fiber pulp with a mass concentration of 10% and a beating degree of 65°SR;
[0113] The plant fiber includes wood fiber and bamboo fiber in a mass ratio of 1:1, and the alkali solution is a potassium hydroxide solution with a mass concentration of 1%;
[0114] b) subjecting the primary fiber slurry to shearing treatment for 5 minutes and then transferring it to a high-pressure homogenizer for homogenization to obtain a secondary fiber slurry;
[0115] The homogenization treatment includes: 4 cycles at a pressure of 40 MPa; 3 cycles at a pressure of 20 MPa; 3 cycles at a pressure of 30 MPa;
[0116] c) stirring the secondary fiber slurry, sodium alginate sol, alkyd resin and talcum powder at 30° C. for 1 hour to obtain a mixed slurry;
[0117] The mass ratio of secondary fiber slurry, sodium alginate sol, alkyd resin and talcum powder is 100:10:5:1;
[0118] The preparation method of sodium alginate sol is as follows: adding tea polyphenols and sodium alginate to acetic acid solution, stirring evenly, adjusting the pH value to 4 with an alkaline solution, and continuing to stir at 50°C for 20 minutes to obtain sodium alginate sol. The mass ratio of tea polyphenols, sodium alginate and acetic acid solution is 0.3:1:100, the mass concentration of acetic acid solution is 0.5%; and the particle size of talc powder is 100-200nm.
[0119] d) sequentially papermaking and drying the mixed slurry to obtain base paper;
[0120] e) sizing and drying the base paper to obtain high-barrier food packaging paper;
[0121] The preparation method of the sizing agent used for sizing comprises:
[0122] Dimethyl sulfoxide was added to alkyd resin, octenylsuccinic anhydride and lauramide propyl betaine, and the mixture was stirred evenly. Modified cellulose and modified cyclodextrin were added in sequence, and the mixture was reacted at 50°C for 10 hours. Propyltrimethoxysilane was then added, and the mixture was stirred at 40°C for 4 hours to obtain a sizing agent. The mass ratio of alkyd resin, octenylsuccinic anhydride, lauramide propyl betaine, propyltrimethoxysilane, modified cellulose and modified cyclodextrin was 1:0.5:0.3:0.05:0.1:0.5.
[0123] The preparation method of modified cellulose and modified cyclodextrin comprises:
[0124] The cellulose suspension and the cyclodextrin suspension were mixed and then ultrasonically treated. After 10 minutes, stearic acid and sodium alginate were added and ultrasonicated. After 10 minutes, the mixture was stirred in a water bath at 60°C for 15 hours, centrifuged and dried to obtain modified cellulose and modified cyclodextrin. The mass concentration of the cellulose suspension was 3%, and the mass concentration of the cyclodextrin suspension was 1%. The mass ratio of the cellulose suspension, the cyclodextrin suspension, the stearic acid and the sodium alginate was 10:90:1:1.
[0125] Example 5
[0126] The production process of high barrier food packaging paper includes the following steps:
[0127] a) mixing plant fiber with alkali solution for reaction, filtering, washing, drying in sequence, adding water and mechanically beating to obtain a primary fiber pulp with a mass concentration of 15% and a beating degree of 70°SR;
[0128] The plant fiber includes wood fiber and bamboo fiber in a mass ratio of 1:1, and the alkali solution is a sodium hydroxide solution with a mass concentration of 5%;
[0129] b) subjecting the primary fiber slurry to shearing treatment for 10 minutes and then transferring it to a high-pressure homogenizer for homogenization to obtain a secondary fiber slurry;
[0130] The homogenization treatment includes: 2 cycles at a pressure of 50 MPa; 1 cycle at a pressure of 30 MPa; 1 cycle at a pressure of 40 MPa;
[0131] c) stirring the secondary fiber slurry, sodium alginate sol, alkyd resin and talcum powder at 40° C. for 0.5 to obtain a mixed slurry;
[0132] The mass ratio of secondary fiber slurry, sodium alginate sol, alkyd resin and talcum powder is 100:20:1:5;
[0133] The preparation method of sodium alginate sol is as follows: adding tea polyphenols and sodium alginate to acetic acid solution, stirring evenly, adjusting the pH value to 6 with an alkaline solution, and continuing to stir at 30°C for 60 minutes to obtain sodium alginate sol. The mass ratio of tea polyphenols, sodium alginate and acetic acid solution is 1:5:100, the mass concentration of acetic acid solution is 1.5%; and the particle size of talc powder is 100-200nm.
[0134] d) sequentially papermaking and drying the mixed slurry to obtain base paper;
[0135] e) sizing and drying the base paper to obtain high-barrier food packaging paper;
[0136] The preparation method of the sizing agent used for sizing comprises:
[0137] N,N-dimethylacetamide was added to alkyd resin, octenylsuccinic anhydride and lauramide propyl betaine, and the mixture was stirred evenly. Then modified cellulose and modified cyclodextrin were added in sequence, and the mixture was reacted at 70°C for 15 hours. Then propyltriethoxysilane was added and stirred at 50°C for 2 hours to obtain a sizing agent. The mass ratio of alkyd resin, octenylsuccinic anhydride, lauramide propyl betaine, propyltriethoxysilane, modified cellulose and modified cyclodextrin was 3:1:0.6:0.1:0.5:0.1.
[0138] The preparation method of modified cellulose and modified cyclodextrin comprises:
[0139] The cellulose suspension and the cyclodextrin suspension were mixed and then subjected to ultrasonic treatment. After 130 minutes, stearic acid and sodium alginate were added and ultrasonic treatment was continued. The mixture was stirred for 10-15 hours in a water bath at 40°C for 30 minutes, and then centrifuged and dried to obtain modified cellulose and modified cyclodextrin. The mass concentration of the cellulose suspension was 1%, and the mass concentration of the cyclodextrin suspension was 3%. The mass ratio of the cellulose suspension, the cyclodextrin suspension, the stearic acid and the sodium alginate was 90:50:2:5.
[0140] Comparative Example 1
[0141] The only difference from Example 1 is step a):
[0142] The beating degree of the primary fiber slurry is 40%.
[0143] Comparative Example 2
[0144] The only difference from Example 1 is step a):
[0145] Plant fibers include only wood fibers.
[0146] Comparative Example 3
[0147] The only difference from Example 1 is step a):
[0148] Plant fibers include only bamboo fibers.
[0149] Comparative Example 4
[0150] The only difference from Example 2 is step b):
[0151] No homogenization was performed.
[0152] Comparative Example 5
[0153] The only difference from Example 2 is step b):
[0154] The homogenization treatment includes 3 cycles at a pressure of 50 MPa and 1 cycle at a pressure of 40 MPa.
[0155] Comparative Example 6
[0156] The only difference from Example 2 is step b):
[0157] The homogenization treatment includes 3 cycles at a pressure of 30 MPa, 2 cycles at a pressure of 40 MPa, and 1 cycle at a pressure of 50 MPa.
[0158] Comparative Example 7
[0159] The only difference from Example 2 is step b):
[0160] The homogenization treatment includes 3 cycles at a pressure of 30 MPa, 2 cycles at a pressure of 50 MPa, and 1 cycle at a pressure of 40 MPa.
[0161] Comparative Example 8
[0162] The only difference from Example 3 is step c):
[0163] The preparation method of sodium alginate sol is as follows: sodium alginate is added to acetic acid solution, stirred evenly, pH value is adjusted to 5 with alkaline solution, and stirring is continued at 40° C. for 30 minutes to obtain sodium alginate sol, wherein the mass ratio of sodium alginate to acetic acid solution is 3:100.
[0164] Comparative Example 9
[0165] The only difference from Example 3 is step c):
[0166] No sodium alginate sol was added to the mixed slurry.
[0167] Comparative Example 10
[0168] The only difference from Example 4 is step e):
[0169] Cellulose and cyclodextrin are not modified, and the mass ratio of alkyd resin, octenyl succinic anhydride, lauramide propyl betaine, methyltriethoxysilane, cellulose, and cyclodextrin is 2:0.7:0.4:0.08:0.3:0.3.
[0170] Comparative Example 11
[0171] The only difference from Example 4 is step e):
[0172] The cellulose is not modified, and the mass ratio of alkyd resin, octenylsuccinic anhydride, lauramide propyl betaine, methyltriethoxysilane, cellulose, and modified cyclodextrin is 2:0.7:0.4:0.08:0.3:0.3.
[0173] Comparative Example 12
[0174] The only difference from Example 4 is step e):
[0175] The cyclodextrin was not modified, and the mass ratio of alkyd resin, octenylsuccinic anhydride, lauramide propyl betaine, methyltriethoxysilane, modified cellulose, and cyclodextrin was 2:0.7:0.4:0.08:0.3:0.3.
[0176] Comparative Example 13
[0177] The only difference from Example 5 is step c):
[0178] No alkyd resin was added, and the mass ratio of the secondary fiber slurry, sodium alginate sol, alkyd resin and talcum powder was 100:10:1.
[0179] Comparative Example 14
[0180] The only difference from Example 5 is step e):
[0181] Octenyl succinic anhydride and lauryl amide propyl betaine were not added. Specifically, dimethyl sulfoxide was added to the alkyd resin, and after stirring evenly, modified cellulose and modified cyclodextrin were added in sequence, and the reaction was carried out at a temperature of 50°C for 10 hours. Then propyltrimethoxysilane was added, and stirred at 40°C for 4 hours to obtain a sizing agent. The mass ratio of alkyd resin, propyltrimethoxysilane, modified cellulose and modified cyclodextrin was 1:0.05:0.1:0.5.
[0182] The high barrier food packaging papers prepared in Examples 1-5 and Comparative Examples 1-14 were tested for tensile strength, tear resistance, oil absorption, water absorption and dustiness according to QB T1014-2010. The results are shown in Table 1.
[0183]
[0184] It can be seen from the experimental data in Table 1 that the high barrier food packaging paper prepared in Examples 1-5 is superior to the high barrier food packaging paper prepared in Comparative Documents 1-14 in terms of tensile strength, tear resistance, oil absorption, water absorption and dustiness.
[0185] Those skilled in the art will appreciate that, although some embodiments described herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the claims of the present application, any one of the claimed embodiments may be used in any combination.
[0186] It should be noted that although the detailed steps of the method of the present application are described in detail above, without departing from the basic principles of the present application, technical personnel in this field can combine, split and change the order of the above steps. The modified technical solution does not change the basic concept of the present application and therefore falls within the scope of protection of the present application.
[0187] So far, the technical solutions of the present application have been described, but it is easy for those skilled in the art to understand that the protection scope of the present application is obviously not limited to these specific implementations. Without departing from the principles of the present application, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present application.
Claims
1. A production process for high barrier food packaging paper, characterized in that: The following steps are involved: a) mixing plant fiber with alkali solution for reaction, filtering, washing, drying in sequence, adding water and mechanically beating to obtain primary fiber slurry; b) subjecting the primary fiber slurry to shearing treatment for 5-10 minutes and then transferring it to a high-pressure homogenizer for homogenization to obtain a secondary fiber slurry; c) stirring the secondary fiber slurry, sodium alginate sol, alkyd resin and talcum powder at 30-40° C. for 0.5-1 h to obtain a mixed slurry; d) sequentially papermaking and drying the mixed slurry to obtain base paper; e) sizing and drying the base paper to obtain high-barrier food packaging paper.
2. The production process according to claim 1, characterized in that: The preparation method of the sodium alginate sol comprises adding tea polyphenols and sodium alginate into an acetic acid solution, stirring evenly, adjusting the pH value to 4-6 with an alkaline solution, and continuing to stir at 30-50° C. for 20-60 minutes to obtain the sodium alginate sol.
3. The production process according to claim 2, characterized in that: The mass ratio of the tea polyphenols, sodium alginate and acetic acid solution is (0.3-1):(1-5):100, and the mass concentration of the acetic acid solution is 0.5-1.5%.
4. The production process according to claim 1, characterized in that: The homogenization process specifically includes: At a pressure of 40-50Mpa, cycle 2-4 times; Under the pressure of 20-30Mpa, cycle 1-3 times; At a pressure of 30-40Mpa, cycle 1-3 times.
5. The production process according to claim 1, characterized in that: The preparation method of the sizing agent used in sizing includes: Add solvent to alkyd resin, octenyl succinic anhydride and lauryl amide propyl betaine, stir evenly, add modified cellulose and modified cyclodextrin in sequence, react at 50-70°C for 10-15h, then add silane coupling agent, stir at 40-50°C for 2-4h to obtain a sizing agent.
6. The production process according to claim 5, characterized in that: The mass ratio of alkyd resin, octenyl succinic anhydride, lauryl amide propyl betaine, silane coupling agent, modified cellulose and modified cyclodextrin is (1-3): (0.5-1): (0.3-0.6): (0.05-0.1): (0.1-0.5): (0.1-0.5).
7. The production process according to claim 5, characterized in that: The preparation method of modified cellulose and modified cyclodextrin comprises: The cellulose suspension and the cyclodextrin suspension are mixed and then subjected to ultrasonic treatment, stearic acid and sodium alginate are then added and ultrasonic treatment is continued, and then stirred for 10-15 hours in a water bath, and modified cellulose and modified cyclodextrin are obtained after centrifugation and drying.
8. The production process according to claim 1, characterized in that: The mass ratio of the secondary fiber slurry, sodium alginate sol, alkyd resin and talcum powder is 100:(10-20):(1-5):(1-5).
9. The production process according to claim 1, characterized in that: The primary fiber slurry has a beating degree of 60-70° SR; and / or The mass concentration of the primary fiber slurry is 10-15%.
10. A high barrier food packaging paper, characterized in that: The product is produced by the production process described in any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of high-strength transparent nanocellulose paper
CN106498795A
Method for realizing micro fiberization of chemical mechanical pulp and for enhancing physical strength of paper
CN107653723A
Preparation method of wrapping paper using dogstail as raw material
CN108086057A
Preparation method for low-quantification waxing-free functional food packaging paper
CN108130797A
High-strength transparent hydrophobic cellulose nano film and preparation method thereof
CN108822315A