Method for testing improved VC (Vitamin C) value of dry and hard cemented sand gravel

Testing the VC value of dry hard cemented gravel through the vibration compactor, the detection problems in the existing technology are solved, the detection accuracy and construction safety are improved, the quality control of cemented gravel dam building materials is ensured, and the indoor and Matching of on-site conditions.

CN118937026APending Publication Date: 2024-11-12HUBEI GEZHOUBA TESTING +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411093589.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to accurately test the VC value of dry hard cemented gravel, especially when the slurry margin is low, the traditional method does not match the on-site construction conditions, resulting in a large difference between the test results and the actual situation, affecting the construction quality. and safe.

Method used

The vibration compactor was used for testing. The time of the vibration head rebound was recorded as the improved VC value through the vibration compactor. The layered filling and insertion of the steel mold collar and the steel mold base plate were used to control the vibration of each layer. The time is 2 to 3 times the modified VC value, ensuring that the sample meets the compressive strength and elastic modulus that meet the design requirements.

Benefits of technology

It improves the scientificity and accuracy of the test, ensures the construction quality and engineering safety of cemented sand and gravel dam building materials, fills the gap in the working detection methods of dry hard cemented sand and gravel at home and abroad, and reduces the risk of accidents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118937026A_ABST
    Figure CN118937026A_ABST
Patent Text Reader

Abstract

The invention provides a method for testing the improved VC value of dry and hard cemented sand gravel, and aims to solve the problem that the existing testing technology is not matched with field construction. According to the method, equipment and programs similar to those of a vibrating compactor in actual construction are adopted, the vibrating compaction time is controlled to the moment when a pressing head bounces back and up, the time serves as the improved VC value of the cemented sand and gravel mixture, and it is ensured that the test result is closer to engineering practice. The test process comprises the steps of wet screening to remove large particles, vibration compaction forming, vibration compaction time recording and the like, and a test mold assembly of a specific specification is adopted. According to the method, the problem of difficulty in traditional VC value test caused by low slurry margin of the poor cemented sand gravel is effectively solved, the scientificity and accuracy of the test are improved, and the compressive strength of the obtained test piece meets the design requirement. The construction efficiency and the engineering quality are improved, and the blank of the dry and hard cemented sand gravel workability detection method at home and abroad is filled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of civil engineering material testing, and in particular relates to a testing method for improved VC value of dry hard cemented gravel. Background Art

[0002] Cemented gravel is a new type of cementing material between concrete and rockfill materials. Cemented gravel (CSGR for short) is between concrete roller-compacted concrete dams and earth-rock dams. Its dam-building materials are a small amount of cementitious materials and gravel and stone materials at the project site, which are mixed, spread, and vibrated to form a material with certain strength and shear resistance. Cemented gravel dam is a new type of dam with strong competitiveness. In my country, many cofferdam projects have adopted cemented gravel dam-building technology. Chinese scholars have called dams with this type of dam-building material "super-poor cementing material dams." Due to the low anti-seepage requirements of cemented gravel in some application scenarios such as mold increase areas and temporary cofferdams, the designed mix ratio has a small amount of cement and water consumption, the slurry material cannot be completely wrapped and filled, and the vibration roller compaction will result in a lack of slurry. The test method of rolled concrete is quite different from the actual situation on site, and the specific parts Figure 1 .

[0003] The cemented gravel used in the mold-increasing area is between a rigid body and a loose body. The on-site construction is close to the loose body process, and the quality inspection is close to the rigid body standard. The VC value test instrument, standard and construction equipment and process are not well matched. Therefore, under different construction conditions, it is necessary to use a test method closer to the actual working conditions to measure the VC value to judge the grindability of the cemented gravel in the mold-increasing area, so as to ensure that the strength, elastic modulus and other indicators of the cemented gravel meet the design requirements. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a test method for the improved VC value of dry hard cemented gravel, aiming to provide a more scientific and reasonable indoor testing technology to better match the on-site construction conditions and ensure the construction quality and engineering safety of cemented gravel dam materials. The improved VC value is applicable to Figure 1 The VC value of concrete refers to the state of half-filling of the slurry, and the VC value of concrete refers to the state of full filling of the slurry. Therefore, the VC value of concrete, which is tested by the slurry overflowing time to see whether it is vibration compacted, is not suitable for cemented gravel, as cemented gravel may not be able to overflow the slurry.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a test method for improved VC value of dry hard cemented gravel, characterized in that: a vibrating compactor is used for testing, and the test steps include: 1) Take the cemented sand and gravel mixture on site, wet screen to remove particles larger than 40 mm and mix thoroughly; 2) Prepare the sample using the vibration compaction method, ensuring that the vibration compaction VC test is completed within 1 hour after mixing; 3) Place the steel mold ring, steel mold and steel mold bottom plate on the solid ground, fill and tamp the mixture in layers; 4) Use a vibrating compactor to compact the material. Record the time when the vibrating compactor starts to rebound. This time is the improved VC value. 5) De-mould the specimen and check the surface compaction status.

[0006] In a preferred embodiment, the basis for determining the improved VC value is the vibration compaction time, that is, the moment when the vibration indenter rebounds, which represents that the sample has reached the vibration compaction state.

[0007] In a preferred embodiment, in step 4), the vibration time of each layer is controlled to be 2 to 3 times of the improved VC value to obtain the compressive strength and elastic modulus that meet the design requirements.

[0008] In a preferred solution, the mixture is divided into four parts before molding, and two parts of the mixture at diagonal positions are grouped as one and loaded into a steel mold for testing. After two tests, the vibration compaction time is the average of the two measured values ​​as the VC value of the cemented sand and gravel mixture.

[0009] In a preferred embodiment, the mixture is molded in two layers, and a wooden stick is used to vibrate the mixture during the single-layer filling process to avoid the concentration or accumulation of aggregates.

[0010] In a preferred embodiment, in the method, the vibration VC test is completed within 1 hour after the mixing in step 1).

[0011] In a preferred embodiment, in step 4), the vibration frequency of the vibration compaction is 28-30 Hz, and the surface static pressure is 0.05-0.15 MPa.

[0012] The present invention effectively addresses the problem of the difficulty in traditional VC value testing of poorly cemented gravel due to low slurry margin, improves the scientificity and accuracy of the test, and the compressive strength of the obtained specimens meets the design requirements. The method is of great significance for indoor testing and quality control of cemented gravel dam materials, improves construction efficiency and engineering quality, and fills the gap in workability testing methods for dry hard cemented gravel at home and abroad.

[0013] The present invention provides a method for testing the improved VC value of dry hard cemented gravel, which has the following beneficial effects by adopting the above method: (1) In view of the problem that it is difficult to accurately obtain the VC value of dry hard cemented gravel materials in traditional tests, the improved VC value test method proposed in the present invention successfully solves this technical problem, so that even poorly cemented gravel with low slurry margin can be accurately evaluated for workability, ensuring the reliability and practicality of the test results; (2) By using a vibrating compactor that is similar in principle to on-site construction machinery to conduct the test, the present invention achieves a high degree of matching between indoor tests and actual construction conditions, improves the consistency between the test results and the actual conditions on the construction site, and ensures that the quality control of cemented gravel dam materials is consistent with the design requirements; (3) Accurately understanding the setting time helps prevent structural safety hazards caused by premature or late setting of materials during construction, ensures the safety of personnel and equipment on the construction site, and reduces the risk of accidents. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 Schematic diagram of cemented gravel material. DETAILED DESCRIPTION

[0015] In actual construction, since cemented gravel is used in some scenarios such as mold-increasing areas and temporary cofferdams, its anti-seepage requirements are relatively low, the designed mix ratio has a small amount of adhesive and water, the slurry material cannot be completely wrapped and filled, and the vibration roller will not cause slurry overflow. The test method of rolled concrete is quite different from the actual situation on site (as shown in the following table) Table 1 Comparison of performance parameters of indoor test equipment

[0016] Table 2 Comparison of performance parameters of on-site rolling equipment

[0017] From the above data, it can be seen that the indoor method of testing VC by rolling concrete does not match the on-site mechanical equipment process. Compared with the vibrating compactor and Vebe consistency meter method (VC value), the surface static pressure of the Vebe consistency meter (VC value) uses a counterweight of 4.9kPa and an exciting force that is far less than that of the vibrating compactor. The rockfill dam construction process is used on site, and the pressure of the rolling work is about 100KPa, which is close to the static pressure of the vibrating compactor. The VC value required for large compaction work (on-site rolling conditions) will be larger or even impossible to measure.

[0018] Example 1 Based on the above situation, the present invention discloses a method for determining the setting time of Guangyuan cemented soil. The test method refers to the "Testing Procedures for Stabilized Materials of Inorganic Binders for Highway Engineering" (JTG E51-2009), and uses a vibrating compactor-molded specimen similar to the principle of on-site construction machinery to test the VC value. The time from the start of vibration to the rebound of the vibration pressure head is the vibration compaction time. At this time, the vibration pressure head no longer sinks, and it is judged that the cemented sand and gravel have reached a compacted state. The time when the pressure head starts to jump, that is, the vibration compaction time, is the VC value of the sample, which is actually consistent with the VC value control principle of roller compacted concrete, as follows: Improved VC value (half-encapsulation theory of cemented gravel) → The pressure head starts to jump up to the VC value (at this time, the sample reaches the vibration compaction state) → Forming compressive strength and elastic modulus, the vibration time of each layer is 2 to 3 times the improved VC value (vibration compaction time); VC value (full-encapsulation theory of cemented gravel) → the VC value is when the pressing plate starts to overflow (at this time the sample reaches a dense state) → the forming compressive strength and elastic modulus, and the vibration time of each layer is 2 to 3 times the VC value (flooding time).

[0019] The specific plan is as follows: A method for testing the improved VC value of dry hard cemented gravel, specifically using a vibrating compactor for testing, the testing steps comprising: 1) Take the cemented sand and gravel mixture on site, wet screen to remove particles larger than 40 mm and mix thoroughly; 2) Prepare the sample using the vibration compaction method, ensuring that the vibration compaction VC test is completed within 1 hour after mixing; 3) Place the steel mold ring, steel mold and steel mold bottom plate on the solid ground, fill and tamp the mixture in layers; 4) Use a vibrating compactor to compact the material. Record the time when the vibrating compactor starts to rebound. This time is the improved VC value. 5) De-mould the specimen and check the surface compaction status.

[0020] In a preferred embodiment, the basis for determining the improved VC value is the vibration compaction time, that is, the moment when the vibration indenter rebounds, which represents that the sample has reached the vibration compaction state.

[0021] In a preferred embodiment, in step 4), the vibration time of each layer is controlled to be 2 to 3 times of the improved VC value to obtain the compressive strength and elastic modulus that meet the design requirements.

[0022] In a preferred solution, the mixture is divided into four parts before molding, and two parts of the mixture at diagonal positions are grouped as one and loaded into a steel mold for testing. After two tests, the vibration compaction time is the average of the two measured values ​​as the VC value of the cemented sand and gravel mixture.

[0023] In a preferred embodiment, the mixture is molded in two layers, and a wooden stick is used to vibrate the mixture during the single-layer filling process to avoid the concentration or accumulation of aggregates.

[0024] Example 2 Based on the scheme described in Example 1, the specific test method parameters are as follows: 1. Material preparation and pretreatment: The cemented gravel material of a certain project design is selected, and its gradation ratio is as shown in Table 1, that is, 150-100 mm, 100-80 mm, 80-60 mm, 60-40 mm, 40-20 mm, 20-5 mm and <5 mm are 18.8%, 6.2%, 8.5%, 13.4%, 17.9%, 15.7% and 19.5% respectively. The recommended mix ratio of C906 is adopted, that is, 40kg cement, 60kg fly ash, 60kg water per cubic meter, 0.45 water-cement ratio, and 2.0kg water reducer (the brand of water reducer is Hengtai), and the mortar margin is ensured to be 0.98 and the mortar margin is 0.96.

[0025] 2. Sample preparation: Take an appropriate amount of cemented sand and gravel mixture on site and use wet screening to remove particles with a size greater than 40 mm to ensure a uniform mixture.

[0026] According to the volume standard, the sample is prepared by vibration compaction method. The vibration compaction VC test shall be completed within 1 hour after mixing, otherwise it will be invalid.

[0027] 3. Trial mold assembly and filling: Use a steel membrane with an inner diameter of 152mm, a height of 170mm, and a wall thickness of 10mm, a steel mold collar with an inner diameter of 152mm, a height of 50mm, and a wall thickness of 10mm, a cylinder gasket with a diameter of 151mm and a thickness of 20mm, and a steel mold base plate with a diameter of 300mm and a thickness of 10mm for assembly.

[0028] Divide the mixed material into four portions according to the quartering method, load two diagonal portions into steel molds, fill in layers and tamp 25 times with a 2cm diameter wooden stick to ensure that the mixture is evenly distributed.

[0029] 4. Vibration compaction: Aim the vibration head of the vibration compactor at the steel mold, start vibration compaction, set the vibration frequency at 28-30Hz, the surface static pressure at about 0.1MPa, and adjust the exciting force to an appropriate range.

[0030] Observe the vibration compaction situation. When the vibration pressure head rebounds, stop vibration immediately and record the time at this time as the improved VC value.

[0031] Result recording and analysis: The average value of the two measured values ​​(accurate to 1s) is recorded as the improved VC value of the sample. In this embodiment, the improved VC value is between 5s and 10s, and the surface of the specimen is compacted and flat without slurry overflow.

[0032] After 90 days of aging, the molded specimens were subjected to a compressive strength test. The results showed that the compressive strength reached the design requirement of 6MPa, and the internal structure of the specimens was uniform, proving that the improved VC value test method effectively guided the construction.

[0033] The method for determining the improved VC value of poorly cemented gravel (semi-encapsulated) by using the above vibration compaction method is only different from the fully encapsulated cemented gravel designed according to the VC value of rolled concrete in the existing guideline SL678-2004 "Technical Guidelines for Dam Construction with Cemented Granular Materials" standard. It is actually consistent with the VC value control principle of rolled concrete, thus solving the method of detecting and evaluating the workability of poorly cemented gravel and achieving the purpose of consistency between indoor and on-site quality control methods.

Claims

1. A test method for the improved VC value of dry hard cemented gravel. Features: The test was carried out using a vibratory compactor. The test steps included: 1) Take the cemented sand and gravel mixture, wet screen to remove particles larger than 40 mm and mix thoroughly to obtain a mixture; 2) Prepare the specimens using the vibration compaction method; 3) Place the steel mold ring, steel mold and steel mold bottom plate on the ground, fill and tamp the mixture in layers; 4) Use a vibrating compactor to compact the material. Record the time when the vibrating compactor starts to rebound. This time is the improved VC value. 5) De-mould the specimen and check the surface compaction state; Complete the test of improved VC value of dry hard cemented gravel.

2. A method for testing the improved VC value of dry hard cemented gravel according to claim 1, Features: The improved VC value is the vibration compaction time, that is, the moment when the vibration indenter rebounds, indicating that the sample has reached the vibration compaction state.

3. A method for testing the improved VC value of dry hard cemented gravel according to claim 1, Features: In the step 4), the vibration time of each layer is controlled to be 2 to 3 times of the improved VC value to obtain the compressive strength and elastic modulus that meet the design requirements.

4. A method for testing the improved VC value of dry hard cemented gravel according to claim 1, Features: In step 3), the mixture is divided into four parts before being molded. Two parts of the mixture at diagonal positions are grouped as one and loaded into a steel mold for testing. After two tests, the vibration compaction time is the average of the two measured values ​​as the VC value of the cemented sand-gravel mixture.

5. A method for testing the improved VC value of dry hard cemented gravel according to claim 1, Features: In the step 3), the mixture is filled into the mold in two layers, and the single-layer filling process is vibrated by wooden sticks to avoid the concentration or accumulation of aggregates.

6. A method for testing the improved VC value of dry hard cemented gravel according to claim 1, Features: In the method, the vibration VC test is completed within 1 hour after the mixing in step 1).

7. A method for testing the improved VC value of dry hard cemented gravel according to claim 1, Features: In the step 4), the vibration frequency of the vibration compaction is 28-30 Hz, and the surface static pressure is 0.05-0.15 MPa.