Simulation test method for annealing process of sheet strip sample

By intermittently controlling the compressive stress before bending of the sample of unloading the plate belt of the air hammer system, the bending problem caused by expansion during the annealing process is solved, and the experimental accuracy and efficiency are improved.

CN118937107APending Publication Date: 2024-11-12ANGANG STEEL CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411023342.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12

Smart Images

  • Figure CN118937107A_ABST
    Figure CN118937107A_ABST
Patent Text Reader

Abstract

The invention provides a thin plate strip sample annealing process simulation test method which is applied to a thermal simulation test machine and comprises the following specific steps: adjusting the loading force of an air hammer on a plate strip sample; mounting a group of plate and strip samples in the same state on a thermal simulation test fixture, performing a plate and strip annealing process test, and collecting stress values of the plate and strip samples; drawing a change curve of the plate and strip sample stress along with time according to a test result; and compiling a test program according to the time when the stress of the plate and strip sample reaches the peak value and the time when the stress is reduced to zero. According to the method, the characteristic that the plate and strip sample is bent due to pressure stress caused by expansion of the plate and strip sample in the heating and heat preservation processes is fully considered, an air hammer system of a thermal simulation testing machine is controlled, the air hammer system is controlled in an intermittent control mode, intermittent tension is applied to the plate and strip sample, and the plate and strip sample is subjected to bending change. The pressure stress on the plate and strip sample is reduced, the expansion of the plate and strip sample due to heating is eliminated, and the bending phenomenon of the plate and strip sample is effectively avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hot processing of steel materials, and in particular to a thin plate strip sample annealing process simulation test method. Background Art

[0002] Generally speaking, the principle of annealing is to heat the material to a certain temperature and then cool it to room temperature at a specified cooling rate. Its main function is to uniformly heat the cold-rolled hard steel coil to the recrystallization annealing temperature, so that the steel grains grow and the plasticity of the strip is improved. In order to study this content, it is necessary to conduct annealing process simulation tests on a series of plate and strip samples.

[0003] In order to develop high-performance cold-rolled products more quickly and efficiently, continuous annealing simulation test machines are generally used to study the relationship between the microstructure and properties of cold-rolled products and the annealing process. The patent number CN200510023266.9, "A strip continuous annealing process simulation device", can continuously simulate the heating, soaking, slow cooling, fast cooling, and aging process of strip samples in a continuous annealing furnace. However, since the strength of the strip sample is low at high temperature, the expansion of the sample during the heating and soaking process will cause the sample to bend and deform. In view of this phenomenon, the invention does not clearly propose effective measures to prevent the deformation of the strip sample. The thermal simulation test machine manufactured by Dynamic Systems of the United States can be equipped with different components or units to complete specific physical simulation experiments, and the strip annealing system is one of them. When using this system to perform a strip annealing process simulation test, a constant tensile force is applied to the two ends of the strip sample by clamping the two ends of the sample, so that the strip sample remains straight due to the action of the tensile force. However, due to the structural characteristics of the system, when the plate strip is in a vacuum state, the main shaft of the clamp that drives the plate strip sample will be subjected to the compressive stress on the plate strip sample caused by the atmospheric pressure. This requires that the force applied to the plate strip sample should be large enough to offset the force of the atmospheric pressure. During the annealing process of the plate strip sample, it is necessary to spray cooling medium on the plate strip sample to cool the plate strip sample, which will destroy the vacuum state of the plate strip sample and weaken the effect of atmospheric pressure on the main shaft of the clamp that drives the plate strip sample, thereby increasing the resultant force on the plate strip sample, and the plate strip is in a tensile state, which can easily cause tensile deformation of the plate strip sample. If the tension applied to both ends of the plate strip sample is too small, the plate strip sample may bend and deform due to thermal expansion. This will eventually affect the experimental accuracy and reduce the experimental efficiency. Summary of the invention

[0004] According to the technical problem raised above, a thin plate strip sample annealing process simulation test method is provided. After the plate strip undergoes continuous annealing process simulation test, the present invention obtains a plate sample with good plate shape, thereby improving the accuracy and efficiency of the experiment.

[0005] The technical means adopted by the present invention are as follows:

[0006] A thin plate strip sample annealing process simulation test method is applied on a thermal simulation test machine, and the specific steps include:

[0007] S1. Adjust the loading force of the air hammer on the plate and strip specimen;

[0008] S2. Install a group of plate and strip samples in the same state on a thermal simulation test fixture, conduct a plate and strip annealing process test, and collect the stress values ​​of the plate and strip samples;

[0009] S3, draw a curve of the change of the stress of the plate and strip specimen over time according to the test results in S2;

[0010] S4. Prepare the test procedure based on the time when the stress of the plate and strip specimen reaches the peak value and the time when the stress drops to zero in S3.

[0011] Furthermore, the step S1 specifically includes:

[0012] Adjust the loading force of the air hammer. The air hammer system drives the main shaft of the testing machine and the fixture on it to move forward and backward, thereby applying tension and pressure to the plate and strip specimen clamped on the fixture;

[0013] Assuming that the pressure of the air hammer is p1, the corresponding cross-sectional area is s1, the external atmospheric pressure is p0, the environmental pressure of the specimen is p2, the cross-sectional area acting on the main shaft of the testing machine is s2, and the friction force of the contact part between the main shaft and the testing machine is f, the resultant force F acting on the specimen through the main shaft of the testing machine is expressed as:

[0014] F=p1s1-(p0-p2)s2-f

[0015] Among them, the plate and strip specimen is subjected to tensile force, F>0.

[0016] Furthermore, the step S2 specifically includes:

[0017] Select a group of plate and strip samples in the same state, install them between the fixtures of the thermal simulation test machine, make the samples straight, start the control program, and conduct the plate and strip annealing process simulation experiment;

[0018] During the test, the force value of the plate and strip sample is collected in real time, and the force condition of the plate and strip sample is observed. When the compressive stress of the plate and strip decreases, the air hammer is turned on to generate tensile stress on the plate and strip sample. During the startup process, the compressive stress of the plate and strip sample gradually decreases until it is reduced to zero, and the plate and strip sample maintains its original straight state. At this time, the air hammer is turned off. As the heating continues, the plate and strip sample will continue to expand, and will be subjected to a certain compressive stress and have a tendency to bend. The force will again experience a process from increase to decrease. Before the force value decreases, the air hammer is started again to generate tensile stress on the plate and strip sample until the compressive stress of the plate and strip sample is reduced to zero, and the plate and strip sample maintains its original straight state. At this time, the air hammer is turned off;

[0019] The above control process is repeatedly performed until the process enters the cooling stage.

[0020] Furthermore, the step S3 specifically includes:

[0021] According to the stress values ​​of the plate and strip sample in the heating and insulation stages in step S2, a curve of the stress change of the plate and strip sample over time is drawn;

[0022] The time when the force reaches the peak value and the time when the force drops from the peak value to zero are marked in the curve. The time when the first plate and strip specimen is subjected to the peak force is recorded as t m1 The time from the peak value to zero is recorded as t Z1 The time corresponding to the second time when the plate and strip specimen stress reaches the peak value is recorded as t m2 The time from the peak value to zero is recorded as t z2 , mark in sequence the time when the plate and strip specimen reaches its peak force and the time when the peak force drops to zero.

[0023] Furthermore, the step S4 specifically includes:

[0024] Prepare the test procedure based on the time when the plate and strip specimens reach the peak force and the time when the peak force drops to zero as determined in S3;

[0025] Elapsed time t m1 Turn on the air hammer system of the thermal simulation test machine to apply tensile stress to the plate and strip specimen. Z1 When t is reached, the air hammer system is turned off to cancel the tensile stress applied to the plate and strip specimen; after a time t m2 The air hammer system of the thermal simulation test machine is turned on again to apply tensile stress to the strip specimen. When the time is t Z2 When the air hammer system is turned off again, the tensile stress applied to the plate and strip specimen is cancelled;

[0026] The air hammer system of the thermal simulation testing machine is repeatedly turned on or off until the program reaches the cooling stage to eliminate the bending caused by the expansion of the plate and strip specimens during the heating or insulation process.

[0027] Compared with the prior art, the present invention has the following advantages:

[0028] The thin plate and strip sample annealing process simulation test method provided by the present invention can unload the compressive stress of the plate and strip sample before bending by reasonably controlling the air hammer system of the thermal simulation test machine, and finally eliminate the expansion of the plate and strip sample due to heat, thereby effectively avoiding the bending of the plate and strip sample and obtaining a plate and strip sample with a good plate shape, which can improve the experimental accuracy and the experimental success rate.

[0029] The thin plate and strip sample annealing process simulation test method provided by the present invention fully takes into account the characteristics of the plate and strip sample being subjected to compressive stress and causing it to bend due to the expansion of the plate and strip sample during the heating and insulation process. By controlling the air hammer system of the thermal simulation test machine and adopting an intermittent control method to control the air hammer system, intermittent tension is applied to the plate and strip sample to reduce the compressive stress on the plate and strip sample. By reasonably controlling the air hammer system of the thermal simulation test machine, the compressive stress before the plate and strip sample bends is unloaded, and finally the expansion of the plate and strip sample due to heat is eliminated, thereby effectively avoiding the bending of the plate and strip sample.

[0030] Based on the above reasons, the present invention can be widely promoted in the field of hot processing technology of steel materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0032] Figure 1 This is a flow chart of the thin plate and strip sample annealing process simulation test method in the present invention. DETAILED DESCRIPTION

[0033] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0034] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0035] like Figure 1 As shown, the present invention provides a thin plate strip sample annealing process simulation test method, which is applied on a thermal simulation test machine, and the specific steps include:

[0036] S1. Adjust the loading force of the air hammer on the plate and strip specimen;

[0037] In specific implementation, as a preferred embodiment of the present invention, the step S1 specifically includes:

[0038] Adjust the loading force of the air hammer. The air hammer system drives the main shaft of the testing machine and the fixture on it to move forward and backward, thereby applying tension and pressure to the plate and strip specimen clamped on the fixture;

[0039] Assuming that the pressure of the air hammer is p1, the corresponding cross-sectional area is s1, the external atmospheric pressure is p0, the environmental pressure of the specimen is p2, the cross-sectional area acting on the main shaft of the testing machine is s2, and the friction force of the contact part between the main shaft and the testing machine is f, the resultant force F acting on the specimen through the main shaft of the testing machine is expressed as:

[0040] F=p1s1-(p0-p2)s2-f

[0041] Among them, the plate and strip specimen is subjected to tensile force, F>0.

[0042] During implementation, in order to prevent F from being too large, which may cause the plate and strip specimen to be subjected to tensile stress and tensile deformation, the F setting range is 10-30 Newtons.

[0043] S2. Install a group of plate and strip samples in the same state on a thermal simulation test fixture, conduct a plate and strip annealing process test, and collect the stress values ​​of the plate and strip samples;

[0044] In specific implementation, as a preferred embodiment of the present invention, step S2 specifically includes:

[0045] Select a group of plate and strip samples in the same state, install them between the fixtures of the thermal simulation test machine, make the samples straight, start the control program, and conduct the plate and strip annealing process simulation experiment;

[0046] During the test, the force value of the plate and strip sample is collected in real time, and the force condition of the plate and strip sample is observed. When the compressive stress of the plate and strip decreases, the air hammer is turned on to generate tensile stress on the plate and strip sample. During the startup process, the compressive stress of the plate and strip sample gradually decreases until it is reduced to zero, and the plate and strip sample maintains its original straight state. At this time, the air hammer is turned off. As the heating continues, the plate and strip sample will continue to expand, and will be subjected to a certain compressive stress and have a tendency to bend. The force will again experience a process from increase to decrease. Before the force value decreases, the air hammer is started again to generate tensile stress on the plate and strip sample until the compressive stress of the plate and strip sample is reduced to zero, and the plate and strip sample maintains its original straight state. At this time, the air hammer is turned off;

[0047] The above control process is repeatedly performed until the process enters the cooling stage.

[0048] S3, draw a curve of the change of the stress of the plate and strip specimen over time according to the test results in S2;

[0049] In specific implementation, as a preferred embodiment of the present invention, step S3 specifically includes:

[0050] According to the stress values ​​of the plate and strip sample in the heating and insulation stages in step S2, a stress variation curve of the plate and strip sample over time is drawn;

[0051] The time when the force reaches the peak value and the time when the force drops from the peak value to zero are marked in the curve. The time when the first plate and strip specimen is subjected to the peak force is recorded as t m1 The time from the peak value to zero is recorded as t Z1 The time when the second plate and strip specimen stress reaches the peak value is recorded as t m2 The time from the peak value to zero is recorded as t z2 , mark in sequence the time when the plate and strip specimen reaches its peak force and the time when the peak force drops to zero.

[0052] S4. Prepare the test procedure based on the time when the stress of the plate and strip specimen reaches the peak value and the time when the stress drops to zero in S3.

[0053] In specific implementation, as a preferred embodiment of the present invention, step S4 specifically includes:

[0054] Prepare the test procedure based on the time when the plate and strip specimens reach the peak force and the time when the peak force drops to zero as determined in S3;

[0055] Elapsed time t m1Turn on the air hammer system of the thermal simulation test machine to apply tensile stress to the plate and strip specimen. Z1 When t is reached, the air hammer system is turned off to cancel the tensile stress applied to the plate and strip specimen; after a time t m2 The air hammer system of the thermal simulation test machine is turned on again to apply tensile stress to the strip specimen. When the time is t Z2 When the air hammer system is turned off again, the tensile stress applied to the plate and strip specimen is cancelled;

[0056] The air hammer system of the thermal simulation testing machine is repeatedly turned on or off until the program reaches the cooling stage to eliminate the bending caused by the expansion of the plate and strip specimens during the heating or insulation process.

[0057] Example 1

[0058] like Figure 1 As shown, the present invention provides a thin plate strip sample annealing process simulation test method. In this embodiment, a sample with a size of 180×50×0.7 mm in length×width×thickness is selected and machined into a steel plate for automobiles, and the following process simulation test procedure is performed:

[0059] On a thermal simulation test machine, the plate and strip sample was heated to 900°C at a heating rate of 10°C / s, kept at this temperature for 3 minutes, and then cooled to room temperature at a cooling rate of 10°C / s. During this process, the force exerted on the plate and strip sample was recorded.

[0060] Adjust the air hammer loading force. Now set the resultant force of the thermal simulation test machine spindle on the sample to 20 Newtons. According to the formula, the air hammer pressure needs to be set to 1.2Mpa.

[0061] Select the above-mentioned strip specimens, take one of them, and install it between the fixtures of the thermal simulation test machine so that the specimen is in a straight state. Start the control program, which is the above-mentioned process simulation experiment program, and conduct the strip annealing process simulation experiment. During the test, collect the stress value of the strip specimen and observe the stress condition of the strip specimen in real time. During the heating or insulation process, the plate and strip sample expands due to heat. At this time, the plate and strip sample is subjected to a certain compressive stress, and the force value gradually increases as the plate and strip sample expands due to heat. When the force value increases to 21.2 kg, press the "Airram" key of the thermal simulation test machine to turn on the air hammer to generate tensile stress on the plate and strip sample until the compressive stress on the plate and strip sample is reduced to zero. Press the "Airram" key of the thermal simulation test machine again to turn off the air hammer. As the plate and strip sample reaches 650℃ and the plate and strip is subjected to 8.3 kg pressure, press the "Airram" key of the thermal simulation test machine to turn on the air hammer to generate tensile stress on the plate and strip sample until the compressive stress on the plate and strip sample is reduced to zero. Press the "Airram" key of the thermal simulation test machine again to turn off the air hammer. Repeat the above control process until the process enters the cooling stage. During the entire process from heating to insulation of the plate and strip sample, the corresponding temperature when the "Airram" key of the thermal simulation test machine is turned on and the stress of the plate and strip sample are shown in Table 1.

[0062] Table 1

[0063] Temperature ℃ Force Kgf 500 21.2 650 8.3 775 3.6 875 1.1 900 0.7 900 0.3

[0064] According to the force values ​​of the plate and strip specimens during the heating and insulation stages, a force-time curve is drawn, and the time corresponding to the force reaching the peak value and the time when the force drops from the peak value to zero are marked on the curve. During the entire process from heating to insulation of the plate and strip specimens, the time corresponding to when the "Airram" key of the thermal simulation test machine is turned on and the force conditions of the plate and strip specimens are shown in Table 2.

[0065] Table 2

[0066]

[0067]

[0068] The test procedure is compiled according to the time when the plate and strip specimens reach the peak force and the time when the peak force drops to zero, as shown in Table 3.

[0069] Table 3

[0070] Time Force Kgf "Airram" key on / off 50 21.2 Open 52 0 closure 65 8.3 Open 67 0 closure 77.5 3.6 Open 79.5 0 closure 87.5 1.1 Open 89.5 0 closure 100 0.7 Open 102 0 closure 130 0.3 Open 132 0 closure

[0071] Example 2

[0072] In this embodiment, a sample of a steel plate for automobile is machined into a size of 180×50×1 mm in length×width×thickness, and the following process simulation experiment procedure is carried out:

[0073] On a thermal simulation test machine, the plate and strip sample was heated to 900°C at a heating rate of 10°C / s, kept at this temperature for 3 minutes, and then cooled to room temperature at a cooling rate of 10°C / s. During this process, the force exerted on the plate and strip sample was recorded.

[0074] Adjust the air hammer loading force. Now set the resultant force of the thermal simulation test machine spindle on the sample to 26 Newtons. According to the formula, the air hammer pressure needs to be set to 1.56Mpa.

[0075] Select the above-mentioned strip specimens, take one of them, and install it between the fixtures of the thermal simulation test machine so that the specimen is in a straight state. Start the control program, which is the above-mentioned process simulation experiment program, and conduct the strip annealing process simulation experiment. During the test, collect the stress value of the strip specimen and observe the stress condition of the strip specimen in real time. During the heating or insulation process, the strip sample expands due to heat. At this time, the strip sample is subject to a certain compressive stress, and the force value gradually increases as the strip sample expands due to heat. When the force value increases to 23.6 kg, press the "Airram" key of the thermal simulation test machine to turn on the air hammer to generate tensile stress on the strip sample until the compressive stress on the strip sample is reduced to zero. Press the "Airram" key of the thermal simulation test machine again to turn off the air hammer. As the strip sample reaches 650℃ and the strip is subjected to 9.2 kg of pressure, press the "Airram" key of the thermal simulation test machine to turn on the air hammer to generate tensile stress on the strip sample until the compressive stress on the strip sample is reduced to zero. Press the "Airram" key of the thermal simulation test machine again to turn off the air hammer. Repeat the above control process until the process enters the cooling stage. During the entire process from heating to insulation of the strip sample, the corresponding temperature when the "Airram" key of the thermal simulation test machine is turned on and the stress of the strip sample are shown in Table 4.

[0076] Table 4

[0077] Temperature ℃ Force Kgf 520 23.6 650 9.2 765 4.3 882 2.1 900 1.1 900 0.6

[0078] According to the force values ​​of the plate and strip specimens during the heating and insulation stages, a force-time curve is drawn, and the time corresponding to the force reaching the peak value and the time when the force drops from the peak value to zero are marked on the curve. During the entire process from heating to insulation of the plate and strip specimens, the time corresponding to when the "Airram" key of the thermal simulation test machine is turned on and the force conditions of the plate and strip specimens are shown in Table 5.

[0079] Table 5

[0080]

[0081]

[0082] The test procedure is compiled according to the time when the plate and strip specimens reach the peak force and the time when the peak force drops to zero, as shown in Table 6.

[0083] Table 6

[0084] Time Force Kgf "Airram" key on / off 52 23.6 Open 54 0 closure 65 9.2 Open 67 0 closure 76.5 4.3 Open 78.5 0 closure 88.5 2.1 Open 91.5 0 closure 106 1.1 Open 108 0 closure 136 0.6 Open 138 0 closure

[0085] The serial numbers of the above embodiments of the present invention are only for description and do not represent the advantages or disadvantages of the embodiments.

[0086] In the above embodiments of the present invention, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0087] In the several embodiments provided in this application, it should be understood that the disclosed technical content can be implemented in other ways. Among them, the device embodiments described above are only schematic. For example, the division of the units can be a logical function division. There may be other division methods in actual implementation. For example, multiple units or components can be combined or integrated into another system, or some features can be ignored or not executed. Another point is that the mutual coupling or direct coupling or communication connection shown or discussed can be through some interfaces, indirect coupling or communication connection of units or modules, which can be electrical or other forms.

[0088] The units described as separate components may or may not be physically separated, and the components shown as units may or may not be physical units, that is, they may be located in one place or distributed on multiple units. Some or all of the units may be selected according to actual needs to achieve the purpose of the present embodiment.

[0089] In addition, each functional unit in each embodiment of the present invention may be integrated into one processing unit, or each unit may exist physically separately, or two or more units may be integrated into one unit. The above-mentioned integrated unit may be implemented in the form of hardware or in the form of software functional units.

[0090] If the integrated unit is implemented in the form of a software functional unit and sold or used as an independent product, it can be stored in a computer-readable storage medium. Based on this understanding, the technical solution of the present invention, in essence, or the part that contributes to the prior art, or all or part of the technical solution can be embodied in the form of a software product, and the computer software product is stored in a storage medium, including a number of instructions for a computer device (which can be a personal computer, a server or a network device, etc.) to perform all or part of the steps of the method described in each embodiment of the present invention. The aforementioned storage medium includes: U disk, read-only memory (ROM, Read-Only Memory), random access memory (RAM, Random Access Memory), mobile hard disk, magnetic disk or optical disk and other media that can store program codes.

[0091] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A thin plate strip sample annealing process simulation test method, applied on a thermal simulation test machine, characterized in that: The specific steps include: S1. Adjust the loading force of the air hammer on the plate and strip specimen; S2. Install a group of plate and strip samples in the same state on a thermal simulation test fixture, conduct a plate and strip annealing process test, and collect the stress values ​​of the plate and strip samples; S3, draw a curve of the change of the stress of the plate and strip specimen over time according to the test results in S2; S4. Prepare the test procedure based on the time when the stress of the plate and strip specimen reaches the peak value and the time when the stress drops to zero in S3.

2. The thin plate strip sample annealing process simulation test method according to claim 1 is characterized in that: The step S1 specifically includes: Adjust the loading force of the air hammer. The air hammer system drives the main shaft of the testing machine and the fixture on it to move forward and backward, thereby applying tension and pressure to the plate and strip specimen clamped on the fixture; Assuming that the pressure of the air hammer is p1, the corresponding cross-sectional area is s1, the external atmospheric pressure is p0, the environmental pressure of the specimen is p2, the cross-sectional area acting on the main shaft of the testing machine is s2, and the friction force of the contact part between the main shaft and the testing machine is f, the resultant force F acting on the specimen through the main shaft of the testing machine is expressed as: F=p1s1-(p0-p2)s2-f Among them, the plate and strip specimen is subjected to tensile force, F>0.

3. The thin plate strip sample annealing process simulation test method according to claim 1 is characterized in that: The step S2 specifically includes: Select a group of plate and strip samples in the same state, install them between the fixtures of the thermal simulation test machine, make the samples straight, start the control program, and conduct the plate and strip annealing process simulation experiment; During the test, the force value of the plate and strip sample is collected in real time, and the force condition of the plate and strip sample is observed. When the compressive stress of the plate and strip decreases, the air hammer is turned on to generate tensile stress on the plate and strip sample. During the startup process, the compressive stress of the plate and strip sample gradually decreases until it is reduced to zero, and the plate and strip sample maintains its original straight state. At this time, the air hammer is turned off. As the heating continues, the plate and strip sample will continue to expand, and will be subjected to a certain compressive stress and have a tendency to bend. The force will again experience a process from increase to decrease. Before the force value decreases, the air hammer is started again to generate tensile stress on the plate and strip sample until the compressive stress of the plate and strip sample is reduced to zero, and the plate and strip sample maintains its original straight state. At this time, the air hammer is turned off; The above control process is repeatedly performed until the process enters the cooling stage.

4. The thin plate strip sample annealing process simulation test method according to claim 1 is characterized in that: The step S3 specifically includes: According to the stress values ​​of the plate and strip sample in the heating and insulation stages in step S2, a stress variation curve of the plate and strip sample over time is drawn; The time when the force reaches the peak value and the time when the force drops from the peak value to zero are marked in the curve. The time when the first plate and strip specimen is subjected to the peak force is recorded as t m1 The time from the peak value to zero is recorded as t Z1 The time corresponding to the second time when the plate and strip specimen stress reaches the peak value is recorded as t m2 The time from the peak value to zero is recorded as t z2 , mark in sequence the time when the plate and strip specimen reaches its peak force and the time when the peak force drops to zero.

5. The thin plate strip sample annealing process simulation test method according to claim 1 is characterized in that: The step S4 specifically includes: Prepare the test procedure based on the time when the plate and strip specimens reach the peak force and the time when the peak force drops to zero as determined in S3; Elapsed time t m1 Turn on the air hammer system of the thermal simulation test machine to apply tensile stress to the plate and strip specimen. Z1 When t is reached, the air hammer system is turned off to cancel the tensile stress applied to the plate and strip specimen; after a time t m2 The air hammer system of the thermal simulation test machine is turned on again to apply tensile stress to the strip specimen. When the time is t Z2 When the air hammer system is turned off again, the tensile stress applied to the plate and strip specimen is cancelled; The air hammer system of the thermal simulation testing machine is repeatedly turned on or off until the program reaches the cooling stage to eliminate the bending caused by the expansion of the plate and strip specimens during the heating or insulation process.

Citation Information

Cited By

  • Method for obtaining straight plate-shaped simulation sample

    CN118821490A

  • A method for obtaining a flat plate-shaped simulated specimen

    CN118821490B