Metallographic detection and reason analysis method for internal defects of medium-thickness plate
Through flaw detection positioning, cutting, grinding and metallographic microscopy detection methods, the complex problem of internal defect detection of medium and thick plates is solved, the detection efficiency and accuracy are improved, the production process is improved, and the product quality is improved.
Patent Information
- Application Number
- CN202411023323.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
During the rolling and production process, the internal defect detection is complex and inefficient due to process instability, and the prior art is difficult to effectively detect and analyze, resulting in damage to product quality.
Using the steps of flaw detection positioning, cutting, grinding, corrosion and metallographic microscopy detection, the defect morphology can be quickly observed and recorded, and the defect type and cause can be determined by cross-segmentation samples, longitudinal offset cutting, diamond grinding and polishing, and shallow corrosion treatment. .
It improves the efficiency and accuracy of internal defect detection of medium and thick plates, improves production process, and improves product quality, which is of great guiding significance.
Smart Images

Figure CN118937336A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of steel industry production method, and in particular, to a metallographic detection and cause analysis method for internal defects of medium and thick plates. Background Art
[0002] During the rolling production process of steel plates, due to the instability of process and production, internal defects are generated, which seriously endanger product quality. Therefore, the detection and cause analysis of internal defects of steel plates is one of the important tasks to improve the process and enhance product quality. The thickness specifications of medium and thick plates are generally 4.5mm to 60mm. Because the steel plates are thick, it is impossible to directly detect their internal defects. Sampling design must be adopted to combine a variety of detection methods to find, detect and analyze defects. The whole process is complicated, the procedures are cumbersome, and the difficulty is relatively high. It is necessary to optimize the entire process of its metallographic detection method to improve the detection efficiency and the accuracy of the results. Summary of the invention
[0003] Based on the above-mentioned technical problems, a metallographic detection and cause analysis method for internal defects of medium and thick plates is provided.
[0004] The technical means adopted by the present invention are as follows:
[0005] A metallographic detection and cause analysis method for internal defects of medium and thick plates, comprising the following steps: S1: cutting a sample, performing flaw detection and positioning on the sample, recording the depth of the defect from the surface, and the length and direction of the defect distribution, placing the defect at the thickness center of the taken metallographic sample, and cross-cutting the sample at the widest point of the defect lateral distribution; S2: cutting the sample, using a wire cutting method, longitudinally offsetting the flaw detection positioning center by 1mm, and making the longitudinal distribution direction of the defect located at the edge of the sample cross section; S3: preparing the sample, grinding the observation surface of the sample where the defect is located, and grinding the sample on 500#, 800#, 1000#, and water sandpaper respectively. Grind, and then polish the test surface on a flannel cloth dipped in diamond grinding paste until the surface is smooth and scratch-free; S4: Corrosion sample, the polished observation surface of the sample is shallowly corroded with an etchant containing HNO3 anhydrous ethanol solution for 1 to 2 seconds, and then washed and dried with hot water at 80 to 100°C; S5: Microscope inspection: Use a metallographic microscope to observe the cross section of the sample, find out the largest defect in the field of view, detect its shape and size, and take photos of the defects in the horizontal and vertical sections respectively; S6: Determine the defect type based on the morphology of the defect and analyze the cause of the defect.
[0006] Further, in the step S1, the sample size is 10-20mm×10-20mm×20-30mm.
[0007] Further, in the step S3, the particle size of the diamond grinding paste is 2.5 μm.
[0008] Further, in the step S3, the polishing time is 1 to 5 minutes.
[0009] Further, in the step S4, the volume percentage of the HNO3 anhydrous ethanol solution is 1% to 2%.
[0010] Compared with the prior art, the present invention has the following advantages:
[0011] The present invention provides a method for metallographic detection and cause analysis of internal defects of medium and thick plates. By adopting flaw detection positioning, the metallographic defect section is selected in a planned manner and corroded for a short time, and the horizontal and vertical microscopic morphology of the internal defects of the steel plate is quickly observed under a metallographic microscope, the type of defect can be accurately determined and the cause of the defect can be analyzed according to its morphology. This improves the efficiency of internal defect detection of medium and thick plates, has important guiding significance for improving production processes and improving product quality, and the method is being continuously applied in product quality inspection and product research and development. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0013] Figure 1 Schematic diagram of inclusion defects in Example 1.
[0014] Figure 2 This is a schematic diagram of the crack defect of Example 2. DETAILED DESCRIPTION
[0015] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0016] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0017] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0018] Unless otherwise specifically stated, the relative arrangement, numerical expressions and numerical values of the parts and steps set forth in these embodiments do not limit the scope of the present invention. Meanwhile, it should be clear that, for ease of description, the sizes of the various parts shown in the accompanying drawings are not drawn according to the actual proportional relationship. The technology, method and equipment known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology, method and equipment should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters represent similar items in the following drawings, and therefore, once a certain item is defined in an accompanying drawing, it does not need to be further discussed in subsequent drawings.
[0019] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by directional words such as "front, back, up, down, left, right", "lateral, vertical, perpendicular, horizontal" and "top, bottom" are usually based on the directions or positional relationships shown in the drawings. They are only for the convenience of describing the present invention and simplifying the description. Unless otherwise specified, these directional words do not indicate or imply that the device or element referred to must have a specific direction or be constructed and operated in a specific direction. Therefore, they cannot be understood as limiting the scope of protection of the present invention: the directional words "inside and outside" refer to the inside and outside relative to the contours of each component itself.
[0020] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used here to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below their position devices or structures". Thus, the exemplary term "above" can include both "above" and "below". The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.
[0021] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. If not otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.
[0022] like Figures 1-2 As shown, the present invention provides a metallographic detection and cause analysis method for internal defects of medium and thick plates, comprising the following steps: S1: cutting a sample, performing flaw detection positioning on the sample, recording the depth of the defect from the surface, and the length and direction of the defect distribution, placing the defect at the thickness center of the taken metallographic sample, and cross-dividing the sample at the widest point of the defect lateral distribution; S2: cutting the sample, using a wire cutting method, longitudinally offsetting the flaw detection positioning center by 1mm, and making the longitudinal distribution direction of the defect located at the edge of the sample cross section; S3: preparing the sample, grinding the observation surface of the sample where the defect is located, and cutting the sample at 500#, 800#, 1000#, and water respectively. Grind on sandpaper, then polish the test surface on flannel dipped in diamond grinding paste until the surface is smooth and scratch-free; S4: Corrode the sample, and shallowly etch the polished observation surface of the sample with an etchant containing HNO3 anhydrous ethanol solution for 1 to 2 seconds, and then wash and dry with hot water at 80 to 100°C; S5: Microscope inspection: Use a metallographic microscope to observe the cross section of the sample, find out the largest defect in the field of view, detect its shape and size, and take photos of the horizontal and vertical cross-sectional defects respectively; S6: Determine the defect type based on the morphology of the defect and analyze the cause of the defect.
[0023] In the step S1, the sample size is 10 to 20 mm×10 to 20 mm×20 to 30 mm.
[0024] In the step S3, the particle size of the diamond grinding paste is 2.5 μm.
[0025] In the step S3, the polishing time is 1 to 5 minutes.
[0026] In the step S4, the volume percentage of the HNO3 anhydrous ethanol solution is 1% to 2%.
[0027] Example 1
[0028] like Figure 1 As shown, it specifically includes the following steps: S1: cutting a sample with a size of about 15mm×15mm×15mm, performing flaw detection on the sample, recording the depth of the defect from the surface, and the length and direction of the defect distribution, placing the defect at the center of the thickness of the metallographic sample, and cross-dividing the sample at the widest point of the defect lateral distribution; S2: cutting the sample, using the wire cutting method, longitudinally offset the flaw detection positioning center by 1mm, and make the longitudinal distribution direction of the defect located at the edge of the sample cross section; S3: preparing the sample, grinding the observation surface of the sample where the defect is located, grinding the sample on 500#, 800#, 1000#, and water sandpaper respectively, and then polishing the test surface on a flannel cloth dipped in 2.5μm diamond grinding paste for 5min, and finally the surface is smooth and scratch-free, as shown in the following figure. Figure 1 ; S5: Microscope inspection: Use a metallographic microscope to observe the cross section of the sample, find out the largest defect in the field of view, detect its shape and size, and take photos and record the defects in the transverse and longitudinal sections respectively; S6: According to the morphology of the defects, the internal defects of medium and thick plates mainly include abnormal inclusions, cracks and holes. According to the morphology of the defects, such as the expansion morphology of the cracks, the size, quantity and distribution characteristics of the inclusions, the defect type is determined and the cause of the defects is analyzed.
[0029] Example 2
[0030] like Figure 2As shown, the specific steps include: S1: cutting a sample with a size of about 15mm×15mm×15mm, detecting and locating the sample, recording the depth of the defect from the surface, and the length and direction of the defect distribution, placing the defect at the thickness center of the metallographic sample, and cross-cutting the sample at the widest point of the defect lateral distribution; S2: cutting the sample, using the wire cutting method, longitudinally offsetting the center of the flaw detection positioning by 1mm, and making the longitudinal distribution direction of the defect located at the edge of the sample cross section; S3: preparing the sample, observing the sample where the defect is located The sample was ground on 500#, 800#, 1000# and water sandpaper respectively, and then polished on a flannel dipped in 2.5μm diamond grinding paste for 5min, until the surface was smooth and scratch-free; S4: Corrosion of the sample, the polished sample observation surface was shallowly corroded with an etchant containing 1% to 2% HNO3 anhydrous ethanol solution by volume for 1 to 2s, and then washed and dried with hot water at 80 to 100°C to obtain the following Figure 2 ; S5: Microscope inspection: Use a metallographic microscope to observe the cross section of the sample, find out the largest defect in the field of view, detect its shape and size, and take photos and record the defects in the transverse and longitudinal sections respectively; S6: According to the morphology of the defects, the internal defects of medium and thick plates mainly include abnormal inclusions, cracks and holes. According to the morphology of the defects, such as the expansion morphology of the cracks, the size, quantity and distribution characteristics of the inclusions, the defect type is determined and the cause of the defects is analyzed.
[0031] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A metallographic detection and cause analysis method for internal defects of medium and thick plates, characterized in that: The method comprises the following steps: S1: cutting a sample, detecting and locating the sample, recording the depth of the defect from the surface, and the length and direction of the defect distribution, placing the defect at the thickness center of the metallographic sample, and cross-dividing the sample at the widest point of the defect lateral distribution; S2: cutting the sample, using a wire cutting method, longitudinally offsetting the center of the flaw detection positioning by 1mm, and making the longitudinal distribution direction of the defect located at the edge of the sample cross section; S3: preparing the sample, grinding the observation surface of the sample where the defect is located, and grinding the sample on 500#, 800#, and 1000# water sandpaper respectively. Grind on the surface, and then polish the test surface on a flannel soaked in diamond grinding paste until the surface is smooth and scratch-free; S4: Corrosion sample, the polished observation surface of the sample is shallowly corroded with an etchant containing HNO3 anhydrous ethanol solution for 1 to 2 seconds, and then washed and dried with hot water at 80 to 100°C; S5: Microscope inspection: Use a metallographic microscope to observe the cross section of the sample, find out the largest defect in the field of view, inspect its shape and size, and take photos of the defects in the horizontal and vertical sections respectively; S6: Determine the defect type based on the defect morphology and analyze the cause of the defect.
2. The method for metallographic detection and cause analysis of internal defects of medium and thick plates according to claim 1 is characterized in that: In the step S1, the sample size is 10-20 mm×10-20 mm×20-30 mm.
3. The metallographic detection and cause analysis method of internal defects of medium and thick plates according to claim 1 is characterized in that: In step S3, the particle size of the diamond grinding paste is 2.5 μm.
4. The metallographic detection and cause analysis method of internal defects of medium and thick plates according to claim 1 is characterized in that: In the step S3, the polishing time is 1 to 5 minutes.