Transmission electron microscope test pretreatment method for carbon quantum dots

By dispersing carbon quantum dots with diluents, the problem of time-consuming observation at high concentrations and low concentrations is solved, and more efficient transmission electron microscopy testing is achieved, reducing the failure rate and detection cycle.

CN118937378AActive Publication Date: 2024-11-12WUHAN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411096350.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-12
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

During the pre-processing process of transmission electron microscopy, the concentration of carbon quantum dots is too low, which causes long time to observe the field of view, or severe agglomeration at high concentrations, resulting in failure of the test, which in turn requires increasing ultrasound power and time to extend the detection cycle.

Method used

The carbon quantum dots are dispersed using diluents (a mixture of water, cosolvents and surfactants), reducing the degree of agglomeration, and even without ultrasonic operation, shortening the time to find the field of view, and improving the degree of dispersion.

Benefits of technology

It reduces the failure rate of transmission electron microscopy test, shortens the detection cycle, improves the testing efficiency, and ensures the accuracy of carbon quantum dot morphology observation and particle size measurement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118937378A_ABST
    Figure CN118937378A_ABST
Patent Text Reader

Abstract

The invention discloses a transmission electron microscope test pretreatment method for carbon quantum dots, and relates to the field of transmission electron microscope detection, and the method comprises the following steps: mixing the carbon quantum dots with a diluent to obtain a dispersion liquid, taking the dispersion liquid, coating the surface of a carbon film with the dispersion liquid, standing, then absorbing liquid on the surface of the carbon film, placing the carbon film under a transmission electron microscope, and searching the visual field of the carbon quantum dots; the diluent is prepared by mixing water, a cosolvent and a surfactant for later use. According to the transmission electron microscope test pretreatment method, the failure rate of the transmission electron microscope test is reduced, the detection period of the transmission electron microscope test is shortened, and the efficiency of the transmission electron microscope test is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of transmission electron microscopy detection, and in particular to a transmission electron microscopy test pretreatment method for carbon quantum dots. Background Art

[0002] The imaging principle of transmission electron microscopy is to project an accelerated and focused electron beam onto a sample. The electrons collide with atoms in the sample and change direction, thereby generating a three-dimensional angle scattering. The size of the scattering angle is related to the density and thickness of the sample, so different images of light and dark can be formed. The image will be displayed on an imaging device (such as a fluorescent screen, film, and photosensitive coupling assembly) after magnification and focusing.

[0003] Carbon quantum dots are a new type of carbon-based nanomaterial. They have diverse physical and chemical properties, good biocompatibility, easy chemical modification, unique optical properties, resistance to photobleaching, rich functional groups (such as amino, hydroxyl, carboxyl), high stability and electron mobility. They have great potential in biological applications such as metal ion detection and bioimaging as fluorescent probes.

[0004] At present, transmission electron microscopy is often used to characterize carbon quantum dots. Before the test, the carbon quantum dots need to be made into a solution and then ultrasonically dispersed, coated on a carbon film, and the field of view where the number of carbon quantum dots meets the observation requirements is found under the transmission electron microscope to complete the pretreatment process, so that the morphology of the carbon quantum dots can be observed under the transmission electron microscope and their particle size can be measured.

[0005] However, during the pretreatment process of the transmission electron microscope test, if the concentration of the carbon quantum dot solution is too low, the number of carbon quantum dots on the carbon film will be small, and it will take a long time to find a field of view that meets the observation quantity requirements under the transmission electron microscope, or even it will be impossible to find a field of view of carbon quantum dots that meets the observation quantity requirements under the transmission electron microscope, resulting in the failure of the transmission electron microscope test; therefore, in order to avoid the problems caused by the low concentration of the carbon quantum dot solution, in actual scientific research, it is often chosen to increase the concentration of the carbon quantum dot solution, but as the concentration of the carbon quantum dot solution increases, the carbon quantum dots are prone to aggregate into clusters, which is not conducive to the observation of the carbon quantum dot morphology and the measurement of the particle size, resulting in the failure of the transmission electron microscope test, thereby requiring the use of higher power conditions for longer ultrasonication during the dispersion process, resulting in an extension of the detection cycle of the transmission electron microscope test. Summary of the invention

[0006] In view of the deficiencies of the above-mentioned related technologies, the present application provides a transmission electron microscopy test pretreatment method for carbon quantum dots. The transmission electron microscopy test pretreatment method of the present application is conducive to reducing the degree of agglomeration of carbon quantum dots under high concentration conditions, thereby reducing the ultrasonic power and ultrasonic time of carbon quantum dots during ultrasonic dispersion, and even eliminating the need for ultrasonic operation. It also shortens the time for finding the field of view of carbon quantum dots. Under the combined effect, the failure rate of transmission electron microscopy testing is reduced, the detection cycle of transmission electron microscopy testing is shortened, and the efficiency of transmission electron microscopy testing is improved.

[0007] The present application provides a carbon quantum dot transmission electron microscopy test pretreatment method using the following technical solution: A transmission electron microscope test pretreatment method for carbon quantum dots comprises the following steps: mixing carbon quantum dots with a diluent to obtain a dispersion, applying the dispersion on a carbon film surface and letting it stand, then absorbing the liquid on the carbon film surface, placing the carbon film under a transmission electron microscope, and finding a field of view for the carbon quantum dots; The diluent includes water, a co-solvent and a surfactant.

[0008] Preferably, the mass volume ratio of the carbon quantum dots to the diluent is 2-3 mg:1 mL.

[0009] Preferably, the mass volume ratio of the carbon quantum dots to the diluent is 2.5 mg:1 mL.

[0010] Preferably, the mixing of the carbon quantum dots with the diluent comprises the following steps: adding the carbon quantum dots to the diluent and vortexing for 0.5-3 minutes.

[0011] Preferably, the mixing of the carbon quantum dots with the diluent comprises the following steps: adding the carbon quantum dots to the diluent and vortexing for 1 minute.

[0012] Preferably, the diluent comprises water and a co-solvent in a volume ratio of 0.5-7:1 and a surfactant in a mass fraction of 0.05-0.2%.

[0013] Preferably, the diluent comprises water and a co-solvent in a volume ratio of 1:1 and a surfactant in a mass fraction of 0.1%.

[0014] Preferably, the diluent is prepared by the following steps: water, a co-solvent and a surfactant are mixed and ultrasonically filtered to obtain the diluent.

[0015] Preferably, the ultrasonic power is 10-80W, and the ultrasonic time is 1-120min.

[0016] Preferably, the ultrasonic power is 50W and the ultrasonic time is 60min.

[0017] Preferably, the filtration comprises filtering through 0.45 μm and 0.22 μm microporous membranes in sequence.

[0018] Preferably, the step of applying the dispersion liquid on the surface of the carbon film and letting it stand comprises the following steps: applying 5-15 μL of the dispersion liquid on the surface of the carbon film and letting it stand for 3-8 minutes.

[0019] Preferably, the step of applying the dispersion liquid on the surface of the carbon film and letting it stand comprises the following steps: applying 10 μL of the dispersion liquid on the surface of the carbon film and letting it stand for 5 minutes.

[0020] Preferably, the co-solvent is one or more of dimethyl sulfoxide, methanol, ethanol, glycerol, formic acid, acetic acid, acetone, tetrahydrofuran and dimethyl ether.

[0021] Preferably, the co-solvent is dimethyl sulfoxide.

[0022] Preferably, the surfactant includes one or both of sodium dodecyl sulfonate and sodium dodecylbenzene sulfonate.

[0023] Preferably, the surfactant is sodium dodecyl sulfate In summary, the present application includes at least one of the following beneficial technical effects: 1. In the pre-treatment process of transmission electron microscopy test, a standby diluent made of water, a co-solvent and a surfactant is introduced to disperse the carbon quantum dots, thereby reducing the degree of agglomeration of the carbon quantum dots under high concentration conditions, thereby reducing the ultrasonic power and ultrasonic time of the carbon quantum dots during ultrasonic dispersion, and even eliminating the need for ultrasonic operation. At the same time, it also shortens the time for finding the field of view of the carbon quantum dots. Under the combined effect, the failure rate of the transmission electron microscopy test is reduced, the detection cycle of the transmission electron microscopy test is shortened, and the efficiency of the transmission electron microscopy test is improved; 2. The dispersion of carbon quantum dots in the field of view during transmission electron microscopy testing is improved, which is conducive to observing and photographing the morphology of carbon quantum dots using transmission electron microscopy and facilitating the measurement of their particle size; 3. The transmission electron microscopy test pretreatment method of the present application is used to observe and measure the particle size of high-concentration carbon quantum dots, which avoids as much as possible the need to reduce the carbon quantum dot concentration to reduce the degree of carbon quantum dot agglomeration, making it difficult to find a field of view where the number of carbon quantum dots meets the observation requirements, resulting in a small number of carbon quantum dots in the field of view, difficult observation, and poor accuracy of particle size statistics. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a transmission electron microscope image obtained using the transmission electron microscope test pretreatment method of Example 1; Figure 2 This is a transmission electron microscope image obtained using the transmission electron microscope test pretreatment method of Example 2; Figure 3This is a transmission electron microscope image obtained using the transmission electron microscope test pretreatment method of Example 3; Figure 4 This is a transmission electron microscope image obtained using the transmission electron microscope test pretreatment method of Example 4; Figure 5 This is a transmission electron microscope image obtained using the transmission electron microscope test pretreatment method of Example 5; Figure 6 This is a transmission electron microscope image obtained using the transmission electron microscope test pretreatment method of Comparative Example 1; Figure 7 This is a transmission electron microscope image obtained using the transmission electron microscope test pretreatment method of Comparative Example 2; Figure 8 This is a transmission electron microscope image obtained using the transmission electron microscope test pretreatment method of Comparative Example 3; Fig. 9 This is a transmission electron microscope image obtained using the transmission electron microscope test pretreatment method of Comparative Example 4; Fig.10 This is a transmission electron microscope image obtained using the transmission electron microscope test pretreatment method of comparative example 5. DETAILED DESCRIPTION

[0025] The present application is further described in detail below in conjunction with examples. The following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. In the following examples, if specific conditions are not specified, they are carried out according to normal conditions or conditions recommended by the manufacturer. The methods used are conventional methods known in the art unless otherwise specified, and the consumables and reagents used are commercially available unless otherwise specified. Unless otherwise specified, the professional and scientific terms used herein have the same meaning as those familiar to those skilled in the art. In addition, any method or material similar or equivalent to the recorded content may also be applied to the present invention.

[0026] The raw materials used in the examples and comparative examples can be obtained from commercial sources. The transmission electron microscope used is a HT7700 transmission electron microscope produced by Hitachi, Japan, and the carbon film used is a common carbon film produced by Beijing Zhongjing Keyi Technology Co., Ltd.

[0027] Preparation Example 1 Preparation Example 1 provides a diluent, and the preparation steps are as follows: use an ultrapure water instrument to prepare ultrapure water, take analytical pure dimethyl sulfoxide and ultrapure water in a volume ratio of 1:1, mix them, and then add sodium dodecyl sulfate, the mass fraction of sodium dodecyl sulfate is 0.1%, and ultrasonicate at a power of 50 W for 60 minutes, and pass through 0.45μm and 0.22μm organic phase microporous filter membranes in turn to remove insoluble impurities that may be mixed in, to obtain a diluent.

[0028] Preparation Example 2 Preparation Example 2 provides a diluent, and the preparation steps are as follows: use an ultrapure water instrument to prepare ultrapure water, take analytical pure dimethyl sulfoxide and ultrapure water in a volume ratio of 1:3, mix them, and then add sodium dodecyl sulfate, the mass fraction of sodium dodecyl sulfate is 0.1%, and ultrasonicate at a power of 50 W for 60 minutes, and pass through 0.45μm and 0.22μm organic phase microporous filter membranes in turn to remove insoluble impurities that may be mixed in, to obtain a diluent.

[0029] Preparation Example 3 Preparation Example 3 provides a diluent, and the preparation steps are as follows: use an ultrapure water instrument to prepare ultrapure water, take analytical pure dimethyl sulfoxide and ultrapure water in a volume ratio of 1:4, mix them, and then add sodium dodecyl sulfate, the mass fraction of sodium dodecyl sulfate is 0.1%, and ultrasonicate at a power of 50 W for 60 minutes, and pass through 0.45μm and 0.22μm organic phase microporous filter membranes in turn to remove insoluble impurities that may be mixed in, to obtain a diluent.

[0030] Preparation Example 4 Preparation Example 4 provides a diluent, and the preparation steps are as follows: use an ultrapure water instrument to prepare ultrapure water, take analytical pure dimethyl sulfoxide and ultrapure water in a volume ratio of 1:7, mix them, and then add sodium dodecyl sulfate, the mass fraction of sodium dodecyl sulfate is 0.1%, and ultrasonicate at a power of 50 W for 60 minutes, and pass through 0.45μm and 0.22μm organic phase microporous filter membranes in turn to remove insoluble impurities that may be mixed in, to obtain a diluent.

[0031] Example 1 Example 1 of the present application provides a method for pre-treatment of carbon quantum dots for transmission electron microscopy testing, the steps of which are as follows: Take 5 mg of carbon quantum dots and 2 mL of the dilution prepared in Preparation Example 1, add the carbon quantum dots to the dilution prepared in Preparation Example 1, and then place it on a vortex instrument and vortex it for 1 min to obtain a dispersion. Use a pipette to draw 10 μL of the dispersion and apply it on the surface of the carbon film. After standing for 5 minutes, use filter paper to absorb the liquid on the surface of the carbon film. Finally, place the carbon film loaded with carbon quantum dots under a transmission electron microscope to find the field of view of carbon quantum dots.

[0032] Example 2 Example 2 of the present application provides a method for pre-treatment of carbon quantum dots for transmission electron microscopy testing. The difference between Example 2 and Example 1 is that the diluent used in Example 2 is the diluent prepared in Preparation Example 2.

[0033] Example 3 Example 3 of the present application provides a method for pre-treatment of carbon quantum dots for transmission electron microscopy testing. The difference between Example 3 and Example 1 is that the diluent used in Example 3 is the diluent prepared in Preparation Example 3.

[0034] Example 4 Example 4 of the present application provides a method for pre-treatment of carbon quantum dots for transmission electron microscopy testing. The difference between Example 4 and Example 1 is that the diluent used in Example 4 is the diluent prepared in Preparation Example 4.

[0035] Example 5 Example 5 of the present application provides a method for pre-treatment of carbon quantum dots for transmission electron microscopy testing, the steps of which are as follows: Take 5 mg of carbon quantum dots and 2 mL of the dilution prepared in Preparation Example 1, add the carbon quantum dots to the dilution prepared in Preparation Example 1, and then ultrasonicate at a power of 50 W for 60 min to obtain a dispersion, use a pipette to draw 10 μL of the dispersion and apply it on the surface of the carbon film. After standing for 5 min, use filter paper to absorb the liquid on the surface of the carbon film, and finally place the carbon film loaded with carbon quantum dots under a transmission electron microscope to find the field of view of carbon quantum dots.

[0036] Comparative Example 1 Comparative Example 1 provides a method for pre-treatment of carbon quantum dots for transmission electron microscopy testing. The difference between Comparative Example 1 and Example 1 is that in Comparative Example 1, the carbon quantum dots are mixed with a mixed solution made of analytically pure dimethyl sulfoxide and ultrapure water in a volume ratio of 1:1.

[0037] Comparative Example 2 Comparative Example 2 provides a method for pre-treatment of carbon quantum dots for transmission electron microscopy testing. The difference between Comparative Example 2 and Example 5 is that in Comparative Example 2, the carbon quantum dots are mixed with a mixed solution made of analytically pure dimethyl sulfoxide and ultrapure water in a volume ratio of 1:1.

[0038] Comparative Example 3 Comparative Example 3 provides a method for pre-treatment of carbon quantum dots for transmission electron microscopy testing. The difference between Comparative Example 3 and Example 2 is that in Comparative Example 3, the carbon quantum dots are mixed with a mixed solution made of analytically pure dimethyl sulfoxide and ultrapure water in a volume ratio of 1:3.

[0039] Comparative Example 4 Comparative Example 4 provides a method for pre-treatment of carbon quantum dots for transmission electron microscopy testing. The difference between Comparative Example 4 and Example 3 is that in Comparative Example 4, the carbon quantum dots are mixed with a mixed solution made of analytically pure dimethyl sulfoxide and ultrapure water in a volume ratio of 1:4.

[0040] Comparative Example 5 Comparative Example 5 provides a method for pre-treatment of carbon quantum dots for transmission electron microscopy testing. The difference between Comparative Example 5 and Example 4 is that in Comparative Example 5, the carbon quantum dots are mixed with a mixed solution made of analytically pure dimethyl sulfoxide and ultrapure water in a volume ratio of 1:7.

[0041] Test and Inspection When the transmission electron microscope test pretreatment methods of Examples 1-5 and Comparative Examples 1-5 were used respectively, transmission electron microscope images were observed and photographed under a transmission electron microscope, as shown in FIG. Figure 1-10 shown.

[0042] Results Analysis The following combination Figure 1-10 The experimental results provided are used to explain this application in detail.

[0043] According to Examples 1-5 and Figure 1-5 It can be seen that in the transmission electron microscope images obtained using the transmission electron microscope test pretreatment method of Examples 1-5, the carbon quantum dots are distributed at a high density within the field of view and have a good degree of dispersion.

[0044] Referring to Examples 1-4, Comparative Example 1 and Comparative Examples 3-5, Figure 1 and Figure 6 , Figure 2 and Figure 8 , Figure 3 and Fig. 9 , Figure 4 and Fig.10 It can be seen that the carbon quantum dots in the field of view in the transmission electron microscope images obtained using the transmission electron microscope test pretreatment method of comparative example 1 and comparative examples 3-5 are severely agglomerated, and it is difficult to observe the morphology of the carbon quantum dots, indicating that the transmission electron microscope test using the transmission electron microscope test pretreatment method of comparative example 1 and comparative examples 3-5 failed. The degree of dispersion of the carbon quantum dots in the field of view in the transmission electron microscope images obtained using the transmission electron microscope test pretreatment method of Examples 1-4 is much higher than the degree of dispersion of the carbon quantum dots in the field of view in the transmission electron microscope images obtained using the transmission electron microscope test pretreatment method of comparative examples 1 and comparative examples 3-5. It shows that the diluent made of dimethyl sulfoxide, ultrapure water and sodium dodecyl sulfate is beneficial to improving the dispersion of carbon quantum dots and inhibiting the agglomeration of carbon quantum dots.

[0045] With reference to Example 5 and Comparative Example 2, Figure 5 and Figure 7 It can be seen that the carbon quantum dots in the field of view in the transmission electron microscope image obtained by the transmission electron microscope test pretreatment method of comparative example 2 are severely agglomerated, and it is difficult to observe the morphology of the carbon quantum dots, indicating that the transmission electron microscope test using the transmission electron microscope test pretreatment method of comparative example 2 failed. The dispersion degree of the carbon quantum dots in the field of view in the transmission electron microscope image obtained by the transmission electron microscope test pretreatment method of embodiment 1 is much higher than the dispersion degree of the carbon quantum dots in the field of view in the transmission electron microscope image obtained by the transmission electron microscope test pretreatment method of comparative example 2. It shows that the diluent made of dimethyl sulfoxide, ultrapure water and sodium dodecyl sulfate is beneficial to improve the dispersion degree of carbon quantum dots and inhibit the agglomeration of carbon quantum dots.

[0046] By comparing Example 1, Example 5, Comparative Example 1 and Comparative Example 2, Figure 1 , Figure 5-7 It can be seen that when the buffer prepared in Preparation Example 1 is mixed with carbon quantum dots during the pretreatment process of the transmission electron microscope test, whether vortex or ultrasound is used, the carbon quantum dots in the field of view in the transmission electron microscope image are evenly dispersed and no agglomeration occurs. Thus, the use of vortex dispersion in the pretreatment process of the transmission electron microscope test shortens the cycle of the pretreatment process of the transmission electron microscope test compared to the use of ultrasound dispersion, and improves the efficiency of the pretreatment of the transmission electron microscope test and the efficiency of the transmission electron microscope test. In the case of mixing the carbon quantum dots with a mixed solution made of analytically pure dimethyl sulfoxide and ultrapure water in a volume ratio of 1:1 during the pretreatment process of the transmission electron microscope test, even if ultrasound is used, under low power and short ultrasound duration, the carbon quantum dots in the field of view of the transmission electron microscope image are still severely agglomerated and difficult to observe and distinguish. It shows that the use of buffer in the pretreatment process of the transmission electron microscope test is conducive to reducing the power and ultrasound duration required for ultrasound, thereby shortening the cycle of the pretreatment process of the transmission electron microscope test, improving the efficiency of the pretreatment of the transmission electron microscope test and the efficiency of the transmission electron microscope test, and can also reduce energy consumption.

[0047] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A method for pre-treatment of carbon quantum dots for transmission electron microscopy testing, characterized in that: The following steps are involved: The carbon quantum dots are mixed with a diluent to obtain a dispersion, the dispersion is applied to the surface of the carbon film and allowed to stand, then the liquid on the surface of the carbon film is removed by suction, and the carbon film is placed under a transmission electron microscope to find the field of view of the carbon quantum dots; The diluent includes water, a co-solvent and a surfactant.

2. The method for pre-treatment of carbon quantum dots for transmission electron microscopy testing according to claim 1, characterized in that: The mass volume ratio of the carbon quantum dots to the diluent is 2-3 mg:1 mL.

3. The method for pre-treatment of carbon quantum dots for transmission electron microscopy testing according to claim 1, characterized in that: The mixing of the carbon quantum dots with the diluent comprises the following steps: adding the carbon quantum dots into the diluent and vortexing for 0.5-3 minutes.

4. The method for pre-treatment of carbon quantum dots for transmission electron microscopy testing according to claim 1, characterized in that: The diluent comprises water and a cosolvent in a volume ratio of 0.5-7:1 and a surfactant in a mass fraction of 0.05%-0.2%.

5. The method for pre-treatment of carbon quantum dots for transmission electron microscopy testing according to claim 1, characterized in that: The diluent is The preparation method comprises the following steps: taking water, a co-solvent and a surfactant, mixing them by ultrasonication and then filtering to obtain the diluent.

6. A method for pre-treatment of carbon quantum dots for transmission electron microscopy testing according to claim 5, characterized in that: The ultrasonic power is 10-80W, and the ultrasonic time is 1-120min.

7. The method for pre-treatment of carbon quantum dots for transmission electron microscopy testing according to claim 5, characterized in that: The filtration includes sequentially passing through 0.45 μm and 0.22 μm microporous membranes.

8. The method for pre-treatment of carbon quantum dots for transmission electron microscopy testing according to claim 1, characterized in that: The step of applying the dispersion liquid on the surface of the carbon film and letting it stand comprises the following steps: applying 5-15 μL of the dispersion liquid on the surface of the carbon film and letting it stand for 3-8 minutes.

9. The method for pre-treatment of carbon quantum dots for transmission electron microscopy testing according to claim 1, characterized in that: The co-solvent includes one or more of dimethyl sulfoxide, methanol, ethanol, glycerol, formic acid, acetic acid, acetone, tetrahydrofuran and dimethyl ether.

10. The method for pre-treatment of carbon quantum dots for transmission electron microscopy testing according to claim 1, characterized in that: The surfactant includes one or both of sodium dodecyl sulfonate and sodium dodecylbenzene sulfonate.

Citation Information

Patent Citations

  • Sample preparation method of small-size carbon dots in transmission electron microscope test

    CN116106342A

  • Amide type carbon quantum dot reinforced foam system as well as preparation method and application thereof

    CN116676078A