Method for rapidly evaluating nutrient release speed of bio-based coated urea

By measuring the water absorption rate of bio-based membrane materials and using the formula y=kx to predict the release period of coated urea, the problems of long detection cycles and coarse results in existing technologies have been solved. This has enabled rapid and accurate evaluation and formulation of membrane materials, and improved the R&D efficiency of slow-release fertilizers.

CN118937593AActive Publication Date: 2024-11-12ANHUI AGRICULTURAL UNIVERSITY +1

Patent Information

Application Number
CN202411124489.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-12
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

In existing technologies, the nutrient release detection methods for bio-based coated urea are characterized by long experimental cycles, complex processes, high costs, and coarse results, making it difficult to achieve accurate evaluation and rapid formulation, resulting in fluctuations in the effectiveness of slow-release fertilizers in different crops and regions.

Method used

By measuring the water absorption rate of the membrane material, the release period of coated urea is predicted using the formula y=kx. The water absorption rate is highly correlated with the nitrogen release period, and the k value is used as a characteristic parameter of nutrient release rate to quickly evaluate the nutrient release speed of the membrane material.

Benefits of technology

This enables rapid and convenient evaluation of urea nutrient release immediately after membrane material synthesis, shortens the new product development cycle, provides precise membrane material formulation and nutrient release design, and improves the development efficiency of slow-release fertilizers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118937593A_ABST
    Figure CN118937593A_ABST
Patent Text Reader

Abstract

The invention discloses a method for rapidly evaluating the nutrient release speed of bio-based coated urea, and relates to the technical field of controlled-release fertilizer coating materials, and the method is realized by preparing a series of biodegradable film materials based on different combinations of different bio-based materials and determining the water absorption rate of the film materials. The method comprises the following steps: mixing and crosslinking a series of different bio-based polyester polyols and isocyanate, curing on a glass plate to form a film, so as to obtain a series of coating materials with certain thicknesses and different nutrient release characteristics, taking a certain mass of a film material for measuring the water absorption rate, and quickly evaluating the nutrient release of the film material on the basis of the nutrient release relationship between the water absorption rate and the coated fertilizer. The method disclosed by the invention is shorter in experiment time, simpler and more convenient in process and low in cost, nutrient release of the coated urea can be evaluated without preparing the coated urea, and a simple and convenient membrane material screening and identifying method is provided for specialization of the coated fertilizer and accurate regulation and control of nutrient release.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of controlled-release fertilizer coating materials, and in particular to a method for rapidly evaluating the properties of bio-based film materials and the corresponding nutrient release speed of coated urea. Background Art

[0002] Polymers, especially polyurethane membranes, have become the main membrane materials for the preparation of coated urea due to their easy film formation and excellent controlled release effect. Bio-based materials have gradually become a research hotspot for the preparation of membrane materials due to their advantages of low price, wide sources, renewable and biodegradable. In recent years, due to factors such as bio-based environmental friendliness and low cost, the technical research and development and product innovation of bio-based polyurethanes have gradually increased, such as castor oil-based polyurethanes, soybean oil-based polyurethanes, linseed oil-based polyurethanes, palm oil-based polyurethanes, rapeseed oil-based polyurethanes, etc. Among many vegetable oils, castor oil-based polyurethanes and soybean oil-based polyurethanes are the most widely used. At present, they have become the main bio-based degradable materials for the preparation of coated slow-release fertilizers. The combination, characteristic evaluation and corresponding coated urea research of bio-oil-based slow-release membrane materials have become hot topics.

[0003] Due to the differences in plant species and soil and hydrothermal conditions in different regions, it is difficult to accurately match the nutrient release of coated urea with the nutrient needs of plants, resulting in fluctuations in the effect of slow-release fertilizers in different crops and different regions. Therefore, the synchronization of nutrient release of slow-release fertilizers and nutrient needs of crops achieved by using different combinations of bio-based degradable materials has always been a concern of the industry. The different sources of coating materials, differences in molecular structure functional groups, and different coating processes after different combinations have a significant impact on the nutrient permeability after film formation. Therefore, different types of bio-based polyester polyols and isocyanates are used for different combinations and composites to construct a series of membrane materials with different nutrient release modes, and to achieve the specialization of coated urea and the important technical path of matching nitrogen supply in fertilizers with crop needs.

[0004] Common methods for detecting and evaluating the nutrient release rate of slow-release fertilizers include water leaching rate method, soil culture method, diffusion and permeability method, electric ultrafiltration method and isotope method, among which the water leaching rate method is the most commonly used method at present, and is also the evaluation method for nutrient release in the national slow-release fertilizer standard (GB / T23348). This method requires the preparation of a series of membrane materials and coated urea products based on the combination of bio-based materials from different sources before it can be implemented. It has the disadvantages of long experimental cycle, complex process, time-consuming and labor-intensive, and high cost. The test results can only roughly evaluate its nutrient release characteristics, which greatly limits the evaluation efficiency of new slow-release membrane materials and is also a bottleneck restricting the research and development and production of special slow-release fertilizers with precise nutrient release. At present, there are few reports on the rapid determination method of nutrient release rate of coated controlled-release fertilizers. The membrane material parameters of some determination methods are not universal, and some are even contrary to the characteristics of the membrane materials. Therefore, technical supervision departments and slow-release fertilizer research and development and production companies are in urgent need of a rapid detection method so that they can quickly detect the characteristic parameters of different membrane materials in a short period of time and estimate the nutrient release law of slow-release fertilizers (urea), thereby realizing the rapid assembly and accurate identification of slow-release coated materials, and providing a method for accurate assembly of membrane materials and rapid evaluation of nutrient release for the development of special slow-release urea. Summary of the invention

[0005] In view of the problems in the prior art, the present invention provides a method for quickly evaluating the nutrient release rate based on measuring the water absorption rate of bio-based membrane materials.

[0006] A method for rapidly evaluating the nutrient release rate of bio-based coated urea, the method comprising:

[0007] S1: Determine the water absorption rate of the membrane material: soak the membrane material with water, measure the weight of the membrane material before and after soaking, record it as M1 and M2, and use the formula

[0008]

[0009] Calculate the water absorption W a ;

[0010] S2: The time when the coating material reaches saturated water absorption is highly correlated with the nitrogen release period. The estimated formula for the release period and saturated water absorption time is:

[0011] y = kx;

[0012] Among them, y is the predicted release period of coated urea, x is the time when the membrane material reaches saturated water absorption, and k is the correlation coefficient between the time when the saturated water absorption of the coating material reaches saturated water absorption and the nitrogen release period, which is obtained by linear fitting;

[0013] The k value is also used as a characteristic parameter of the nutrient release rate. The larger the k value, the slower the nutrient release rate of the coated urea, and the smaller the k value, the faster the nutrient release rate of the coated urea.

[0014] Preferably, the membrane material is a polymer formed by combining bio-based polyester polyol and isocyanate.

[0015] Preferably, k=1.94.

[0016] Preferably, the error between y and the actual release period of the corresponding bio-based coated urea does not exceed 14 days.

[0017] Preferably, the membrane material is prepared in the following manner:

[0018] (1) mixing the bio-based polyester polyol and the isocyanate, and mixing them on a high-speed disperser for 20 to 50 seconds to obtain a homogeneous mixed liquid;

[0019] (2) Pour the mixed solution onto a clean and dry glass plate, and evenly spread the mixed solution on the glass plate using a coating rod with a thickness of 80 μm to form a coating film layer;

[0020] (3) Place the coated glass plate in an infrared drying oven at 40-60°C for curing. When the surface of the coating film is cured and no longer sticky, increase the temperature of the infrared drying oven to 70-80°C for curing. Take it out after 20-40 minutes and transfer it to an oven at 50-60°C for further curing until the coating film is completely cured to form a film with stable strength. Remove the film from the glass plate.

[0021] Furthermore, the coating material was placed in an oven at 50° C. and dried for 24 hours.

[0022] Furthermore, the dried coating material is placed in a balance for weighing, and 0.5 g of the coating material is taken out. The mass of the coating material at this time is recorded as M1. If it is less than 0.5 g, errors may easily occur, and if it is too large, the test cost may be increased.

[0023] Furthermore, the weighed membrane material is placed in a beaker filled with deionized water to be completely soaked.

[0024] Furthermore, the beaker containing the membrane material and deionized water is placed in a constant temperature incubator set at 25°C.

[0025] Furthermore, after the immersion time was 1, 3, 7, 10, and 14 days, the membrane material was taken out every 7 days and the residual water on the membrane surface was absorbed by filter paper. At this time, the membrane was weighed and recorded as M2.

[0026] Furthermore, after weighing the infiltrated membrane material, the membrane material is put back into the beaker containing deionized water, and the infiltration is continued until the weight of the membrane material no longer changes, and the infiltration time when the water absorption rate is saturated is recorded.

[0027] The time for the membrane material to reach the saturated water absorption rate is the time from when the membrane material begins to be infiltrated by water to when the mass of the infiltrated membrane material no longer changes.

[0028] Compared with the prior art, the present invention has at least the following beneficial effects:

[0029] The water absorption rate of the membrane material in the present invention can be measured after the membrane material is synthesized, not after the coated urea is separated. Compared with the traditional nutrient determination, a faster and simpler evaluation method is provided for the nutrient release of the coated urea, that is, the speed of nutrient release can be determined according to the water absorption rate before the urea is coated, and the release period can be preliminarily determined, and subsequently, the coated urea that meets the expected release period can be produced by designing different ratios of membrane material water absorption rates or different membrane thicknesses;

[0030] The present invention provides technical support for the combination of special film materials and the design of nutrient patterns of coated urea that matches crop needs, realizes relatively accurate design of nutrient release of film materials and coated urea, and shortens the research and development cycle of new special slow-release fertilizer products. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0032] Figure 1 The water absorption rate of different membrane materials changes with the immersion time;

[0033] Figure 2 The nitrogen cumulative release rate diagram of urea coated with different membrane materials;

[0034] Figure 3 7-day nitrogen release rate of urea coated with different membrane materials;

[0035] Figure 4 Fitting curves of water absorption of different membrane materials and nitrogen cumulative release rate of coated urea;

[0036] Figure 5 Fitting curve of water absorption of different membrane materials and 7-day nitrogen release rate of coated urea. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be clearly and completely described in combination with the drawings in the embodiments of the present invention. In order to better reveal the law of change of water absorption rate, the selected membrane materials are all membrane materials with specific thickness prepared by coating with controllable thickness coating rod.

[0038] Example 1

[0039] A method for quickly evaluating the nutrient release rate of bio-based coated urea is as follows:

[0040] (1) Determination of water absorption rate of membrane materials: Take 0.5g of the dried bio-based raw material (small molecule castor oil polyester polyol: large molecule castor oil polyester polyol: isocyanate = 5.5:0.5:4) to prepare the membrane material (codenamed A1), put it into a beaker filled with deionized water to completely soak it, and place it in a 25°C constant temperature box. After soaking for 1, 3, 7, 10, and 14 days, use filter paper to absorb the residual water on the membrane every 7 days. At this time, weigh the membrane and calculate its water absorption performance, and record the time to reach saturated water absorption. The water absorption rate calculation formula is as follows:

[0041]

[0042] Where: Wa is the water absorption rate; M2 is the weight of the film after infiltration; M1 is the weight of the dry film.

[0043] (2) Controlled release performance test: The film material formula selected in the above embodiment was used to prepare a polyurethane coated urea sample by drum granulation and spraying process, and the coating thickness was 3.0%. Determination of nutrient release of coated urea: Weigh 10.00g of controlled release fertilizer and put it into a small bag made of 100 mesh nylon gauze. After sealing, put the small bag into a 250mL plastic bottle, add 200mL distilled water, cover and seal, and place it in a 25°C incubator. Sampling time 1, 7, 14, 21 days after every 7 days, until the nutrient dissolution rate reaches more than 80%, it is considered to be completely released. When sampling, turn the glass bottle upside down 3 times to make the liquid concentration in the bottle consistent, and then take out about 40ml of liquid from the bottle and put it into a small glass bottle for nitrogen determination. Then, pour out all the remaining liquid in the bottle, add 200mL distilled water again, seal and put it into the incubator for further cultivation. Nitrogen dissolution rate: Nitrogen is measured by Kjeldahl method.

[0044] Example 1 The water absorption rate of the membrane material, the cumulative nitrogen release rate of the coated urea after static water extraction, and the 7-day nitrogen release rate are recorded as follows, as shown in Table 1 below.

[0045] Table 1: Determination data of water absorption rate of membrane material and nutrient release of coated urea in Example 1

[0046] Time / Day Water absorption (%) Cumulative release rate (%) 7-day release rate (%) 1 0.72 0.05 0.05 3 1.30 0.32 / 7 1.70 0.41 0.36 10 1.48 1.02 / 14 2.03 1.68 1.27 21 2.25 3.69 2.01 28 2.54 6.82 3.13 35 2.64 11.77 4.95 42 2.94 17.85 6.08 49 3.15 26.58 8.73 56 3.14 35.26 8.68 63 3.55 41.60 6.34 70 3.52 48.08 6.48 77 3.25 53.82 5.74 84 58.57 4.75 91 62.82 4.25 98 66.26 3.44 105 69.87 3.61 112 73.10 3.23 119 75.82 2.72 126 77.93 2.11 133 80.19 2.26

[0047] Example 2

[0048] A method for quickly evaluating the nutrient release rate of bio-based coated urea is as follows:

[0049] (1) Determination of water absorption rate of membrane materials: Take 0.5g of membrane materials (codenamed A2) made of different dried bio-based raw material combinations (small molecule castor oil polyester polyol, castor oil polyester polyol: isocyanate = 3:3:4), put them into beakers filled with deionized water and completely soak them, and place them in a constant temperature box at 25°C. After soaking for 1, 3, 7, 10, and 14 days, use filter paper to absorb the residual water on the membrane every 7 days. At this time, weigh the membrane and calculate its water absorption performance, and record the time to reach saturated water absorption. The water absorption rate calculation formula is as follows:

[0050]

[0051] Where: Wa is the water absorption rate; M2 is the weight of the film after infiltration; M1 is the weight of the dry film.

[0052] (2) Same as Example 1.

[0053] Example 2 The water absorption rate of the membrane material, the cumulative nitrogen release rate of the coated urea after static water extraction, and the 7-day nitrogen release rate are recorded as follows, as shown in Table 2 below.

[0054] Table 2: Determination data of water absorption rate of membrane material and nutrient release of coated urea in Example 2

[0055]

[0056]

[0057] Example 3

[0058] A method for quickly evaluating the nutrient release rate of bio-based coated urea is as follows:

[0059] (1) Determination of water absorption rate of membrane materials: Take 0.5g of dried membrane material (codenamed A3) made of another bio-based raw material combination (epoxidized soybean oil polyester polyol: isocyanate = 6.5:3.5), put it into a beaker filled with deionized water and completely soak it, and place it in a constant temperature box at 25°C. After soaking for 1, 3, 7, 10, and 14 days, use filter paper to absorb the residual water on the membrane every 7 days. At this time, weigh the membrane and calculate its water absorption performance, and record the time to reach saturated water absorption. The water absorption rate calculation formula is as follows:

[0060]

[0061] Where: Wa is the water absorption rate; M2 is the weight of the film after infiltration; M1 is the weight of the dry film.

[0062] (2) Same as Example 1.

[0063] Example 3 The water absorption rate of the membrane material, the cumulative nitrogen release rate of the coated urea after static water extraction, and the 7-day nitrogen release rate are recorded as follows, as shown in Table 3 below.

[0064] Table 3: Determination data of water absorption rate of membrane material and nutrient release of coated urea in Example 3

[0065]

[0066]

[0067] The water absorption performance related curves of Examples 1-3 are as follows Figure 1 The relevant release curve data are shown as Figure 2 and Figure 3 The water absorption saturation time and the coated urea release period data of Examples 1-3 are shown in Table 4 below. To further illustrate the relationship between water absorption rate and nutrient release, the water absorption rate and nutrient release measurement data were fitted, and the relevant curve is shown in Figure 4 , Figure 5 And as shown in Table 5.

[0068] Table 4 Water absorption and release period measurement data of Examples 1-3

[0069] Membrane Time to reach water absorption saturation / day Release period / day Example 1 63 133 Example 2 56 105 Example 3 35 56

[0070] Table 5 Fitting relationship between the time to reach saturated water absorption (x) and the release period (y) of Examples 1-3

[0071] Relational Correlation coefficient y=1.94x 0.987

[0072] The results show that: under the condition of a certain film thickness, the nutrient release law of the coated urea of ​​the three different bio-based film materials is highly consistent with the water absorption rate change law of the three film materials, and the order of water absorption rate and nutrient release is: A3 film>A2 film>A1 film. The water absorption rate of the film material increases with the extension of the immersion time. When the water absorption rate is close to saturation, the nutrient release rate of the coated urea also reaches the maximum, indicating that the water absorption rate of the film material can be used as an indicator of the nutrient release rate of the bio-based coated urea. The results also show that the nutrient release period of the bio-based coated urea is close to twice the time it takes for the film material to reach saturated water absorption, and the relationship between the two is extremely significantly correlated. Among them, the maximum difference between the time it takes for the coating material to reach saturated water absorption and the release period of the coated urea is only 14 days.

[0073] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for rapidly evaluating the nutrient release rate of bio-based coated urea, characterized in that: The method comprises: S1: Determine the water absorption rate of the membrane material: soak the membrane material with water, measure the weight of the membrane material before and after soaking, record it as M1 and M2, and use the formula Calculate the water absorption W a ; S2: The time when the coating material reaches saturated water absorption is highly correlated with the nitrogen release period. The estimated formula for the release period and saturated water absorption time is: y = kx; Among them, y is the predicted release period of coated urea, x is the time when the membrane material reaches saturated water absorption, and k is the correlation coefficient between the time when the saturated water absorption of the coating material reaches and the nitrogen release period, which is obtained by linear fitting; The k value is also used as a characteristic parameter of the nutrient release rate. The larger the k value, the slower the nutrient release rate of the coated urea, and the smaller the k value, the faster the nutrient release rate of the coated urea.

2. A method for rapidly evaluating the nutrient release rate of bio-based coated urea according to claim 1, characterized in that: The membrane material is a polymer formed by combining bio-based polyester polyol and isocyanate.

3. A method for rapidly evaluating the nutrient release rate of bio-based coated urea according to claim 2, characterized in that: The k=1.

94.

4. The method for rapidly evaluating the nutrient release rate of bio-based coated urea according to claim 1, characterized in that: The membrane material is prepared in the following manner: (1) mixing the bio-based polyester polyol and the isocyanate, and mixing them on a high-speed disperser for 20 to 50 seconds to obtain a homogeneous mixed liquid; (2) Pour the mixed solution onto a clean and dry glass plate, and evenly spread the mixed solution on the glass plate using a coating rod with a thickness of 80 μm to form a coating film layer; (3) Place the coated glass plate in an infrared drying oven at 40-60°C for curing. When the surface of the coating film is cured and no longer sticky, increase the temperature of the infrared drying oven to 70-80°C for curing. Take it out after 20-40 minutes and transfer it to an oven at 50-60°C for further curing until the coating film is completely cured to form a film with stable strength. Remove the film from the glass plate.

5. The method for rapidly evaluating the nutrient release rate of bio-based coated urea according to claim 1, characterized in that: The M1 is 0.5g.

6. The method for rapidly evaluating the nutrient release rate of bio-based coated urea according to claim 1, characterized in that: During wetting, the water submerges the membrane material.

7. A method for rapidly evaluating the nutrient release rate of bio-based coated urea according to claim 1, characterized in that: The soaking temperature was 25°C.

8. A method for rapidly evaluating the nutrient release rate of bio-based coated urea according to claim 1, characterized in that: The time for the membrane material to reach the saturated water absorption rate is the time from when the membrane material begins to be infiltrated by water to when the mass of the infiltrated membrane material no longer changes.

Citation Information

Patent Citations

  • Method for testing field nutrient release regulation of urea formaldehyde slow-release fertilizer

    CN104541726A

  • Method for predicting nitrogen releasing amount of parabolic type resin-coated controlled-release urea in greenhouse soil

    CN105528508A

  • Rapid detection method for slow release period of polyurethane coated urea fertilizer, and applications thereof

    CN107367471A

  • Accurate controlled release membrane material and application thereof

    CN115490560A

  • Release Capsule, Polymeric Solution, Method of Producing Capsules, Encapsulated Urea for Use in Soil Correction, Polymeric Material for Release of a Release Compound, Polymeric Controlled Release System, Method of Controlled Release, Application Composition and Soil Repairing Agent

    US20240043353A1

Cited By

  • Method for evaluating slow release property of polyurethane coated urea based on infrared spectroscopic analysis