Manufacturing method of lens assembly and lens assembly

By depositing refractive layers of titanium pentoxide or tantalum pentoxide and magnesium fluoride on the lens, and preventing oxidation through oxygen extraction, the problem of high cost of anti-reflective film preparation in the prior art is solved, and an efficient lens assembly is achieved manufacture.

CN118938362APending Publication Date: 2024-11-12VIVO MOBILE COMM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410999935.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the preparation cost of the anti-reflective film is relatively high, and the coating process is complicated, making it difficult to improve the manufacturing efficiency.

Method used

Titanium pentoxide or tantalum pentoxide is used as the first film material and magnesium fluoride is used as the second film material. By depositing and extracting oxygen on the lens to prevent oxidation of magnesium fluoride, a refractive layer is formed, which simplifies the coating process and reduces costs. .

Benefits of technology

The manufacturing cost of the reflective film is effectively reduced, the manufacturing efficiency is improved, the refractive index is increased, the imaging effect of the lens assembly is ensured, and the coating process is simplified.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118938362A_ABST
    Figure CN118938362A_ABST
Patent Text Reader

Abstract

The invention discloses a manufacturing method of a lens assembly and the lens assembly, and the manufacturing method of the lens assembly comprises the steps: depositing a first film material on a lens, so as to form a first refraction layer on the lens; oxygen on the surface of the first refraction layer is extracted; a second film material is deposited on the first refraction layer to form a second refraction layer on the first refraction layer, and the refractive index of the first refraction layer is larger than that of the second refraction layer; wherein the first film material comprises trititanium pentoxide or tantalum pentoxide, and the second film material comprises magnesium fluoride.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of lens assemblies, and in particular relates to a manufacturing method of a lens assembly and a lens assembly. Background Art

[0002] The camera in a mobile phone is composed of multiple lenses made of glass or plastic. When strong light enters the camera, the inside of the lens will reflect the light multiple times. Most of the light passes through the lens to form an image on the image sensor, but some of the light returns through the image sensor and then passes through the lens and flat glass to form an image again. The image at this time is called a ghost image.

[0003] In the related art, ghosting is improved by coating an anti-reflection film on the inner surface of the lens. Currently, the coating process of the anti-reflection film is relatively complicated, so it is difficult to improve the manufacturing efficiency of the anti-reflection film. Summary of the invention

[0004] The present application aims to provide a method for manufacturing a lens assembly and a lens assembly, which at least solves the problem of high preparation cost of anti-reflection film in the related art.

[0005] In order to solve the above technical problems, this application is implemented as follows:

[0006] In a first aspect, an embodiment of the present application provides a method for manufacturing a lens assembly, comprising:

[0007] Depositing a first film material on the lens to form a first refractive layer on the lens;

[0008] Extracting oxygen from the surface of the first refractive layer;

[0009] Depositing a second film material on the first refractive layer to form a second refractive layer on the first refractive layer, wherein the refractive index of the first refractive layer is greater than the refractive index of the second refractive layer;

[0010] The first film material includes titanium pentoxide or tantalum pentoxide, and the second film material includes magnesium fluoride.

[0011] In a second aspect, an embodiment of the present application provides a lens assembly, which is manufactured by the manufacturing method in the first aspect, and includes:

[0012] lens;

[0013] A first refractive layer is provided on the lens;

[0014] A second refractive layer is disposed on the first refractive layer, and the refractive index of the first refractive layer is greater than the refractive index of the second refractive layer;

[0015] The first refractive layer is formed by depositing a first film material, the first film material includes titanium pentoxide or tantalum pentoxide, and the second refractive layer is formed by depositing a second film material, the second film material includes magnesium fluoride.

[0016] In a third aspect, an embodiment of the present application provides a camera module, including:

[0017] As the lens assembly in the second aspect.

[0018] In a fourth aspect, an embodiment of the present application provides an electronic device, including:

[0019] Such as the camera module in the third aspect.

[0020] In the embodiment of the present application, when the first refractive layer is plated, oxygen needs to be filled into the first film material to improve the absorption of titanium pentoxide or tantalum pentoxide, and magnesium fluoride and oxygen will undergo an oxidation reaction, that is, magnesium oxide is generated, and the refractive index increases, thereby causing the spectrum to shift. Therefore, in this embodiment, an air extraction layer is added between the first refractive layer and the second refractive layer to extract the oxygen that has not been ionized in the first refractive layer, prevent the oxidation of magnesium fluoride, avoid the increase in the refractive index of the second refractive layer, and ensure the imaging effect of the lens assembly.

[0021] In the related art, the reflective film on the lens is made of three materials, so that the reflective film is not easy to change the refractive index of the lens component. In this embodiment, when two coating materials are used, considering the problem that magnesium fluoride may be affected by oxidation, the oxidation of magnesium fluoride is avoided by extracting oxygen, thereby avoiding the increase of the refractive index of the second refractive layer. In this case, it is not necessary to make the reflective film with three materials, which reduces the materials used for the reflective film and reduces the manufacturing cost of the reflective film. In addition, by reducing the coating materials of the reflective film, the coating process of one of the materials can be saved, thereby simplifying the coating process and improving the manufacturing efficiency of the reflective film.

[0022] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0024] Figure 1 is a flow chart of a method for manufacturing a lens assembly according to an embodiment of the present application;

[0025] Figure 2 is a partial schematic diagram of a lens assembly according to an embodiment of the present application;

[0026] Figure 3is a schematic structural diagram of an electronic device according to an embodiment of the present application;

[0027] Figure 4 The picture is shown when the lens assembly of the electronic device in the related art is not provided with an inner coating;

[0028] Figure 5 The picture taken when the lens assembly of the electronic device in the related art is provided with an internal coating is shown;

[0029] Figure 6 shows a picture taken by an electronic device in an embodiment of the present application;

[0030] Figure 7 is a graph showing the variation of static pressure with displacement in a lens assembly according to an embodiment of the present application;

[0031] Figure 8 is a graph showing the change of reflectivity with wavelength at an incident angle of 0° and an incident angle of 30° according to an embodiment of the present application;

[0032] Fig. 9 is a curve diagram showing the variation of transmittance with wavelength at an incident angle of 0° and an incident angle of 30° according to an embodiment of the present application;

[0033] Fig.10 is a graph showing how the refractive index and extinction coefficient vary with wavelength in a lens assembly according to an embodiment of the present application;

[0034] Fig.11 is one of the structural schematic diagrams of the lens assembly according to an embodiment of the present application;

[0035] Fig.12 This is the second structural schematic diagram of the lens assembly according to the embodiment of the present application.

[0036] Reference numerals:

[0037] 200 lens assembly, 210 lens, 211 window area, 212 non-window area, 220 first refractive layer, 230 second refractive layer, 240 anti-fingerprint coating, 250 external coating, 260 ink layer, 300 optical adhesive layer, 270 polyethylene terephthalate layer, 280 shadowless adhesive, 290 coating, 310 CD pattern area. DETAILED DESCRIPTION

[0038] The embodiments of the present application will be described in detail below. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and should not be construed as limitations on the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.

[0039] The term "first" or "second" in the specification and claims of this application may include one or more of the features explicitly or implicitly. In the description of this application, unless otherwise specified, "plurality" means two or more. In addition, "and / or" in the specification and claims means at least one of the connected objects, and the character " / " generally means that the objects connected before and after are in an "or" relationship.

[0040] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0041] Combine the following Figure 1-Figure 12 The present invention describes a manufacturing method of a lens assembly, a lens assembly, a camera module and an electronic device according to embodiments of the present application.

[0042] like Figure 1 As shown, the manufacturing method of the lens assembly according to some embodiments of the present application includes:

[0043] Step 102, depositing a first film material on the lens to form a first refractive layer on the lens;

[0044] Step 104, extracting oxygen from the surface of the first refractive layer;

[0045] Step 106, depositing a second film material on the first refractive layer to form a second refractive layer on the first refractive layer, wherein the refractive index of the first refractive layer is greater than the refractive index of the second refractive layer, wherein the first film material comprises titanium pentoxide or tantalum pentoxide, and the second film material comprises magnesium fluoride.

[0046] In an embodiment of the present application, the film layer in contact with the lens is a first refractive layer, and the coating material of the first refractive layer is titanium pentoxide or tantalum pentoxide. A second refractive layer is arranged on the first refractive layer, and the coating material of the second refractive layer is magnesium fluoride. The refractive index of titanium pentoxide or tantalum pentoxide is relatively high, and the refractive index of magnesium fluoride is relatively low. When plating the first refractive layer, the first film material needs to be filled with oxygen to improve the absorption of titanium pentoxide or tantalum pentoxide, and magnesium fluoride and oxygen will undergo an oxidation reaction, that is, magnesium oxide is generated, and the refractive index increases, thereby causing the spectrum to shift. Therefore, in this embodiment, an air extraction layer is added between the first refractive layer and the second refractive layer to extract the unionized oxygen in the first refractive layer, prevent the oxidation of magnesium fluoride, avoid the increase in the refractive index of the second refractive layer, and ensure the imaging effect of the lens assembly.

[0047] In the related art, the reflective film on the lens is made of three materials, so that the reflective film is not easy to change the refractive index of the lens component. In this embodiment, when two coating materials are used, considering the problem that magnesium fluoride may be affected by oxidation, the oxidation of magnesium fluoride is avoided by extracting oxygen, thereby avoiding the increase of the refractive index of the second refractive layer. In this case, it is not necessary to make the reflective film with three materials, which reduces the materials used for the reflective film and reduces the manufacturing cost of the reflective film. In addition, by reducing the coating materials of the reflective film, the coating process of one of the materials can be saved, thereby simplifying the coating process and improving the manufacturing efficiency of the reflective film.

[0048] In some embodiments, optionally, after the step of depositing the second film material on the first refractive layer, the manufacturing method further comprises: returning to the step of depositing the first film material on the second refractive layer until the number of layers of the first refractive layer and the second refractive layer reaches a set number of layers.

[0049] That is, after the step of depositing the second film material on the first refractive layer, the manufacturing method further comprises: sequentially depositing the first film material and the second film material on the second refractive layer until the number of layers of the first refractive layer and the second refractive layer reaches a set number of layers.

[0050] After the first refractive layer and the second refractive layer are formed on the lens in sequence, the first film material is continuously deposited on the second refractive layer, thereby forming the first refractive layer on the second refractive layer, and then the second film material is deposited on the newly formed first refractive layer, thereby forming the second refractive layer on the newly formed first refractive layer. Therefore, one side of the lens is sequentially formed with: the first refractive layer, the second refractive layer, the first refractive layer, the second refractive layer, and so on, until the number of the first refractive layer and the second refractive layer reaches the set number of layers, for example, the number of the first refractive layer and the number of the second refractive layer both reach 3 layers, and the step of continuing to deposit the first film material is stopped. When the number of the first refractive layer and the second refractive layer is small, the coating formed by the first refractive layer and the second refractive layer has an effective effect of weakening the ghost image. When the number of the first refractive layer and the second refractive layer is large, the stress of the coating is large, and the lens is easy to break when the lens assembly falls. Therefore, when the set number of layers is determined, the effect of weakening the ghost image can be guaranteed, and the probability of the lens breaking can be reduced. In this embodiment, the set number of layers is 3 layers. In other embodiments, the set number of layers is not limited to 3 layers.

[0051] In some embodiments, optionally, the first film material further includes: aluminum oxide.

[0052] High refractive index materials include titanium pentoxide and tantalum pentoxide, among which tantalum pentoxide is more expensive, while titanium pentoxide is cheaper and has a stable evaporation rate. Titanium pentoxide thin film grows in layers and has a high aggregation density, so the stress is relatively large, while aluminum oxide grows in columns, has a large porosity, and has low film stress. Therefore, the high refractive index material uses a certain proportion of aluminum oxide doped in titanium pentoxide to obtain a titanium-aluminum mixture that meets the requirements of low stress, high refractive index, and no absorption.

[0053] B=λ max / λ min , B represents the low reflectivity bandwidth (λ max is the maximum wavelength in the low reflection region, λ min is the minimum wavelength in the low reflection region), L is the refractive index of the outermost film, D = n H -n L , D is defined as: the difference in high refractive index except the outermost layer, n H The refractive index of the high-refractive-index material, n L It represents the refractive index of the low-refractive-index material, and T is the total optical thickness of the first refractive layer plus the second refractive layer, expressed in multiples of the average wavelength.

[0054] in, R ave (B, L, T, D) is used to represent the average reflectivity. According to the above functional relationship, to obtain a lower average reflectivity, D must be larger, L must be as small as possible, and T must be as large as possible. Based on cost and stability, two materials are used for design.

[0055] As the proportion of aluminum oxide increases, the refractive index of the titanium-aluminum mixture decreases, the porosity increases, and the stress decreases. As the proportion of titanium pentoxide increases, the refractive index increases and the stress increases. Finally, the ratio of titanium pentoxide to aluminum oxide is determined to be 9:1, and the oxygen filling amount is 120sccm. By testing the transmittance and reflectivity of the titanium-aluminum mixture single layer film, and using the MacLeod software to calculate the optical constants of the titanium-aluminum mixture, such as Fig.10 As shown, where n represents the refractive index and k represents the extinction coefficient.

[0056] The material with the lowest refractive index at present is magnesium fluoride, whose refractive index in the 550nm band is 1.38, and based on the above theoretical analysis, the low refractive index material should be magnesium fluoride.

[0057] In a possible application, the outward side of the lens is also provided with a coating, and the outward side of the lens is provided with a hard anti-reflection film, and the high refractive index material is Si3N4 with a refractive index of 1.95 to 2.05 and the low refractive index material is SiO2 with a refractive index of 1.60 to 1.70. x N y , using optical thin film design software to complete the design of hard anti-reflection film, by adjusting SiO x N y The refractive index is determined by the gas filling ratio of Si3N4. In order to meet the hardness and reflectivity indicators, the refractive index of Si3N4 is finally determined to be 2.02. x N y The refractive index is 1.63, the average reflectivity from 420nm to 680nm is less than 1.2%, the nanoindentation hardness is 15.5GPa, and the total thickness of the film is 1150nm. The specific process parameters are as follows:

[0058]

[0059] Table 1

[0060]

[0061] Table 2

[0062] This embodiment can use only two coating materials, the high refractive index material is titanium pentoxide, and the low refractive index material is magnesium fluoride. The uniformity of the two materials can be corrected respectively by two correction baffles of the evaporator. Products can be placed in the inner and outer circles, which can improve the production capacity. The number of film layers is 6, the total thickness of the film layer is 245nm, and the coating time is 90min. The production capacity is significantly improved. Taking a circular lens with a diameter of 30mm as an example, compared with the anti-reflection film in the related technology, the production capacity is increased by about 30%, and the cost is low and the process preparation is simpler.

[0063] This embodiment adopts optical thin film technology and utilizes thin film interference to reduce the residual reflection on the glass surface, as shown in Table 3, the reflectivity and transmittance standards of the internal and external coatings.

[0064]

[0065]

[0066] Table 3

[0067] In some embodiments, optionally, the coating device includes an ion source, a correction baffle, and a coating material baffle. Before the step of forming the first refractive layer on the lens, the manufacturing method further includes: controlling the operation of the ion source, the correction baffle, and the coating material baffle; opening the ion outlet of the ion source, and performing ion source assisted coating on the first film material through the ions flowing out of the ion outlet.

[0068] The deposition of the first film material is assisted by an ion source, which is beneficial to improving the deposition effect of the first film material and the compactness of the first refractive layer. The first refractive layer is not easy to absorb moisture, thereby ensuring the structural stability of the first refractive layer.

[0069] In some embodiments, optionally, before the step of depositing the second film material on the first refractive layer, the manufacturing method further comprises: closing the ion outlet.

[0070] After being bombarded by ions, magnesium fluoride loses fluorine and its refractive index increases. Therefore, during the deposition of the second film material on the first refractive layer, the ion outlet is kept closed to prevent the ion source from affecting the deposition effect of magnesium fluoride.

[0071] During the deposition of the second film material, the ion outlet is closed and ions cannot be discharged from the ion outlet; however, the ion source is always in operation.

[0072] The startup time of the ion source is relatively long. If the ion source is turned off before depositing the second film material, when the first film material needs to be deposited, a long time is required to wait for the ion source to start, resulting in a longer coating time.

[0073] Therefore, the ion source is kept in a normally open state. When depositing the first film material, the ion outlet is opened, and when depositing the second film material, the ion outlet is closed. This can not only prevent the ion source from affecting the deposition effect of magnesium fluoride, but also save the time waiting for the ion source to be turned on, thereby saving coating time and improving coating efficiency.

[0074] In some embodiments, optionally, before the step of depositing the second film material on the first refractive layer, the manufacturing method further comprises: increasing the temperature of the lens coating environment to a set temperature.

[0075] After magnesium fluoride is bombarded by ions, it will lose fluorine and its refractive index will increase. If no ion source is added to assist in the deposition of magnesium fluoride, the density of the film will be poor and it will easily absorb moisture (high temperature and humidity, boiling water, salt spray testing, etc.), which will also cause the spectrum to shift.

[0076] Therefore, before depositing the second film material, the temperature of the coating environment is increased, that is, the ambient temperature of the lens assembly is processed to the set temperature. By increasing the temperature, the density of magnesium fluoride is increased, and the problem of magnesium fluoride absorbing water is solved. The final film layer stacking structure is shown in Table 4, and the process parameters are shown in Table 5.

[0077]

[0078] Table 4

[0079]

[0080] Table 5

[0081] like Figure 8 As shown in FIG. 1 , a curve diagram showing the reflectivity changes with wavelength at 0° incidence and 30° incidence is shown. Fig. 9 As shown, a graph showing the variation of transmittance with wavelength at 0° incidence and 30° incidence is shown.

[0082] Adding ion source to assist the plating of magnesium fluoride will cause magnesium fluoride to lose fluorine and increase absorption, which will affect the overall transmittance of the lens assembly. This embodiment solves the problem of magnesium fluoride absorption by increasing the empty layer vacuum and heating to assist deposition, that is, by increasing the temperature in the coating chamber to increase the density of magnesium fluoride, the problem of magnesium fluoride absorbing water is solved. The specific process is shown in Table 6:

[0083]

[0084] Table 6

[0085] The coating scheme of this embodiment is that the film layer can pass the high temperature and high humidity test for 48 hours, the salt spray test for 48 hours, the ultraviolet test for 96 hours, etc., and the film layer will not peel off, crack, or have different colors, and the transmittance of the ring test will not decrease.

[0086] In some embodiments, optionally, after the number of the first refractive layer and the second refractive layer reaches a set number of layers, the manufacturing method further includes: laminating a film on the lens, wherein the film avoids the first refractive layer and the second refractive layer.

[0087] During the coating process on the lens, in order to improve the density of magnesium fluoride, the coating environment needs to reach a set temperature. The temperature of the environment in which the lens assembly is located is relatively high. However, the film that needs to be bonded to the lens is likely to bubble in a high temperature environment. Therefore, in order to avoid the problem of film bubbling, the present embodiment adopts a solution of coating first and then bonding the film, which can not only improve the density of magnesium fluoride, but also avoid bubbling of the film due to heat, which is beneficial to improving the quality of the lens assembly.

[0088] In some embodiments of the present application, Figure 2 As shown, a lens assembly 200 is proposed. The lens assembly 200 is made by the manufacturing method in any of the above embodiments. The lens assembly 200 includes: a lens 210, a first refractive layer 220 and a second refractive layer 230. The first refractive layer 220 is arranged on the lens 210, and the second refractive layer 230 is arranged on the first refractive layer 220. The refractive index of the first refractive layer 220 is greater than the refractive index of the second refractive layer 230. The first refractive layer 220 is formed by depositing a first film material, and the first film material includes titanium pentoxide or tantalum pentoxide. The second refractive layer 230 is formed by depositing a second film material, and the second film material includes magnesium fluoride. The second film material is deposited after oxygen on the surface of the first refractive layer 220 is extracted.

[0089] In the embodiment of the present application, the film layer in contact with the lens 210 is the first refractive layer 220, and the coating material of the first refractive layer 220 is trititanium pentoxide or tantalum pentoxide. The second refractive layer 230 is arranged on the first refractive layer 220, and the coating material of the second refractive layer 230 is magnesium fluoride. The refractive index of trititanium pentoxide or tantalum pentoxide is relatively high, and the refractive index material of magnesium fluoride is relatively low. When plating the first refractive layer 220, the first film material needs to be filled with oxygen to improve the absorption of trititanium pentoxide or tantalum pentoxide, and magnesium fluoride and oxygen will undergo an oxidation reaction, that is, magnesium oxide is generated, and the refractive index increases, thereby causing the spectrum to shift. Therefore, in this embodiment, by adding an air extraction layer between the first refractive layer 220 and the second refractive layer 230, the oxygen that has not been ionized in the first refractive layer 220 is extracted to prevent the oxidation of magnesium fluoride, avoid the increase of the refractive index of the second refractive layer 230, and ensure the imaging effect of the lens assembly 200.

[0090] In the related art, the reflective film on the lens 210 is made of three materials, so that the reflective film is not easy to change the refractive index of the lens assembly 200. In this embodiment, when two coating materials are used, considering the problem that magnesium fluoride may be affected by oxidation, the oxidation of magnesium fluoride is avoided by extracting oxygen, thereby avoiding the increase of the refractive index of the second refractive layer 230. In this case, it is not necessary to make the reflective film with three materials, which reduces the materials used for the reflective film and reduces the manufacturing cost of the reflective film. In addition, by reducing the coating materials of the reflective film, the coating process of one of the materials can be saved, thereby simplifying the coating process and improving the manufacturing efficiency of the reflective film.

[0091] In some embodiments, optionally, the number of the first refractive layer 220 and the second refractive layer 230 are both multiple layers, and the first refractive layers 220 and the second refractive layers 230 are alternately stacked and distributed.

[0092] After the first refractive layer 220 and the second refractive layer 230 are sequentially formed on the lens 210, the first film material is continuously deposited on the second refractive layer 230, thereby forming the first refractive layer 220 on the second refractive layer 230, and then the second film material is deposited on the newly formed first refractive layer 220, thereby forming the second refractive layer 230 on the newly formed first refractive layer 220. Therefore, one side of the lens 210 is sequentially formed with: the first refractive layer 220, the second refractive layer 230, the first refractive layer 220, the second refractive layer 230, and so on, until the number of the first refractive layer 220 and the second refractive layer 230 reaches a set number of layers, for example, the number of the first refractive layer 220 and the number of the second refractive layer 230 both reach 3 layers, and the step of continuing to deposit the first film material is stopped. When the number of the first refractive layer 220 and the second refractive layer 230 is small, the coating formed by the first refractive layer 220 and the second refractive layer 230 is effective in weakening the ghost image. When the number of the first refractive layer 220 and the second refractive layer 230 is large, the stress of the coating is large, and when the lens assembly 200 falls, the lens 210 is easy to break. Therefore, when the number of layers is determined, the effect of weakening the ghost image can be guaranteed and the probability of the lens 210 breaking can be reduced.

[0093] like Figure 3 As shown, a lens assembly 200 is provided on the camera of the electronic device, such as Figure 4 As shown, when the lens assembly in the related art is not provided with an inner coating, the ghosting effect is obvious in the dotted frame. Figure 5 As shown, when an inner coating is provided on the lens assembly in the related art, the ghosting effect in the dotted frame is weakened, but the ghosting still has a great impact on the image quality. Figure 6 As shown, when an inner coating is provided on the lens assembly 200 in this embodiment, the ghosting effect in the dotted frame is weak.

[0094] In some embodiments, optionally, the sum of the thicknesses of the multi-layer first refraction layer 220 and the multi-layer second refraction layer 230 is W, and 240 nm≤W≤600 nm.

[0095] By reducing a coating material, the thickness of the coating can be effectively reduced. While satisfying the anti-reflection effect of the coating, the thickness of the coating on the lens 210 can be controlled within the range of 240nm≤W≤600nm. The stress of the coating is low and it is not easy to cause the lens 210 to break.

[0096] Illustratively, W may be 240 nm, 260 nm, or 600 nm.

[0097] In some embodiments, optionally, the number n1 of the first refractive layer 220 satisfies, n1≥3; the number n2 of the second refractive layer 230 satisfies, n2≥3.

[0098] The number of the first refractive layer 220 and the second refractive layer 230 is the same. When the number of the first refractive layer 220 and the second refractive layer 230 both reaches 3 layers, the coating formed on the lens 210 has a better anti-reflection effect.

[0099] In some embodiments, optionally, the first refraction layer 220 further includes: aluminum oxide.

[0100] High refractive index materials include titanium pentoxide and tantalum pentoxide, among which tantalum pentoxide is more expensive, while titanium pentoxide is cheaper and has a stable evaporation rate. Titanium pentoxide thin film grows in layers and has a high aggregation density, so the stress is relatively large, while aluminum oxide grows in columns, has a large porosity, and has low film stress. Therefore, the high refractive index material uses a certain proportion of aluminum oxide doped in titanium pentoxide to obtain a titanium-aluminum mixture that meets the requirements of low stress, high refractive index, and no absorption.

[0101] In some embodiments, optionally, based on the first refractive layer 220 including titanium pentoxide, the mass ratio of titanium pentoxide to aluminum oxide is 9:1; based on the first refractive layer 220 including tantalum pentoxide, the mass ratio of tantalum pentoxide to aluminum oxide is 9:1.

[0102] Taking the first refractive layer 220 including titanium pentoxide as an example, as the proportion of aluminum oxide increases, the refractive index of the titanium-aluminum mixture decreases, the porosity increases, and the stress decreases. When the proportion of titanium pentoxide increases, the refractive index increases and the stress increases. When the mass ratio of titanium pentoxide to aluminum oxide is 9:1, the refractive index of the coating is higher and the stress is lower, which is beneficial to improving the quality of the lens assembly 200.

[0103] In some embodiments, optionally, a window area 211 and a non-window area 212 are provided on the lens 210, a portion of the first refractive layer 220 and a portion of the second refractive layer 230 cover the window area 211, and another portion of the first refractive layer 220 and another portion of the second refractive layer 230 extend to the non-window area 212.

[0104] Light can pass through the window area 211 on the lens 210, and the first refractive layer 220 and the second refractive layer 230 both cover the window area 211, ensuring that the light reflected by the image sensor is not easy to pass through the window area 211, thereby avoiding the ghost phenomenon. The first refractive layer 220 and the second refractive layer 230 both extend to the non-window area 212, so that the first refractive layer 220 and the second refractive layer 230 cover the transition position between the window area 211 and the non-window area 212, preventing the light reflected by the image sensor from passing through the transition position between the window area 211 and the non-window area 212, further avoiding the occurrence of ghost phenomena.

[0105] In a possible application, the processing scheme of the lens assembly 200 can adopt the following two methods:

[0106] The first one is the solution of bonding the film to the glass.

[0107] The inner surface coating of the lens 210 of this embodiment needs to be heated, and the film (the structure composed of the optical adhesive layer 300 + the polyethylene terephthalate layer 270 + the shadowless adhesive 280 is called the film) is not resistant to high temperature. Therefore, when the lens 210 adopts the film and glass bonding solution process, it is necessary to coat the inner surface of the embodiment with the film first and then bond the film. The specific implementation process is as follows:

[0108] Membrane segment: membrane → electroplating (plating layer 290) → silk screen printing ink → laser cutting (cutting out the window area 211).

[0109] Glass section: silk screen ink layer 260 → outer coating → coating (inner coating in this embodiment) → film lamination → bubble removal.

[0110] like Fig.11 As shown, an outer coating 250 and an inner coating (a first refractive layer 220 and a second refractive layer 230 are alternately stacked) are arranged on the lens, an anti-fingerprint coating 240 is arranged on the outer coating 250, and an ink layer 260, an optical adhesive layer 300, a polyethylene terephthalate layer 270, a shadowless adhesive 280 layer, a coating layer 290 and an ink layer 260 are sequentially stacked on the non-window area of ​​the lens.

[0111] The second method is to etch the CD pattern.

[0112] The stacked structure of the CD pattern etching scheme in this embodiment is as follows Fig.12 As shown, the process flow is as follows: glass→etching CD pattern→screen printing ink layer 260→electroplating→deplating→screen printing ink layer 260→coating outer layer→coating (inner coating in this embodiment).

[0113] like Fig.12As shown, an outer coating 250 and an inner coating (a first refractive layer 220 and a second refractive layer 230 are alternately stacked) are arranged on the lens, an ink layer 260 is arranged on the non-window area of ​​the lens, a CD grain area 310 is arranged on the non-window area, and a coating 290 is arranged on the ink layer 260 corresponding to the CD grain area 310.

[0114] The lens assembly 200 manufactured in the above manner has the advantage of high strength. The lens 210 with GG7i glass as the substrate and the outer coating 250 structure remain unchanged. The coating structure of this embodiment is adopted, and the static pressure of the lens 210 is 24kg. Figure 7 As shown, the strength is only reduced by 20%, which can effectively reduce the market failure risk of the lens 210 being broken.

[0115] The lens assembly 200 manufactured in the above manner has the following advantages:

[0116] First, the total thickness of the film layer is 245nm, and the stress of the film layer is low. Compared with the strengthened glass, the static pressure is only reduced by 20%, which can increase the sandpaper drop height of the whole machine and reduce market failure.

[0117] Second, the anti-reflection film of this embodiment reduces the residual reflectivity of the inner surface of the lens 210 and increases the transmittance, thereby improving the imaging quality.

[0118] Third, the total thickness of the inner coating solution of this embodiment is 245nm, which is basically consistent with the thickness of the inner coating in the related art and will not increase the production cost.

[0119] Fourth, the internal coating solution of the present application uses only two coating materials, which is more conducive to mass production and has better spectral consistency.

[0120] Fifth, the bonding solution of the glass lens 210 according to the process of this embodiment can solve the problem that the film is not resistant to high temperatures.

[0121] Sixth, the coating scheme of this embodiment is that the film layer can pass high temperature and high humidity test for 48 hours, salt spray test for 48 hours, ultraviolet test for 96 hours, etc., and the film layer will not peel off, crack, discolor, etc., and the transmittance of the ring test will not decrease.

[0122] Seventh, the coating solution of this embodiment can effectively reduce ghosting in strong light photography and improve image quality.

[0123] It should be noted that the inner coating and outer coating 250 solutions mentioned in the above embodiment refer to AR (Anti-Reflection Glass) coating.

[0124] The inner coating solution of this embodiment has a non-absorbing film layer and can replace the inner coating in the related art. As shown in Table 7, the inner surface coating comparison of the lens 210 is shown.

[0125]

[0126] Table 7

[0127] In an embodiment of the present application, a camera module is proposed, comprising: a lens assembly as in any of the above embodiments. The camera module in this embodiment can achieve the technical effects of the lens assembly as in any of the above embodiments, which will not be repeated here.

[0128] In an embodiment of the present application, an electronic device is proposed, including: a camera module as in the above embodiment. The electronic device in this embodiment can achieve the technical effect of the camera module as in the above embodiment, which will not be repeated here.

[0129] In one possible application, the electronic device may be a mobile phone, a tablet computer, a camera, a drone, etc.

[0130] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0131] Although the embodiments of the present application have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the claims and their equivalents.

Claims

1. A method for manufacturing a lens assembly, characterized in that: The manufacturing method comprises: Depositing a first film material on the lens to form a first refractive layer on the lens; Extracting oxygen from the surface of the first refractive layer; Depositing a second film material on the first refractive layer to form a second refractive layer on the first refractive layer, wherein the refractive index of the first refractive layer is greater than the refractive index of the second refractive layer; Wherein, the first film material includes titanium pentoxide or tantalum pentoxide, and the second film material includes magnesium fluoride.

2. The manufacturing method according to claim 1, characterized in that: After the step of depositing a second film material on the first refractive layer, the manufacturing method further comprises: The first film material and the second film material are sequentially deposited on the second refractive layer until the number of layers of the first refractive layer and the second refractive layer both reach a set number of layers.

3. The manufacturing method according to claim 1, characterized in that: The first film material also includes: aluminum oxide.

4. The manufacturing method according to any one of claims 1 to 3, characterized in that: Before the step of forming the first refractive layer on the lens, the manufacturing method further comprises: Control ion source operation; The ion outlet of the ion source is opened, and the ions flowing out of the ion outlet perform ion source assisted plating on the first film material.

5. The manufacturing method according to claim 4, characterized in that: Before the step of depositing the second film material on the first refractive layer, the manufacturing method further comprises: The ion outlet is closed.

6. A lens assembly, characterized in that: The lens assembly is manufactured by the manufacturing method according to any one of claims 1 to 5, and the lens assembly comprises: lens; A first refractive layer, disposed on the lens; A second refractive layer is disposed on the first refractive layer, and the refractive index of the first refractive layer is greater than the refractive index of the second refractive layer; The first refractive layer is formed by depositing a first film material, the first film material includes titanium pentoxide or tantalum pentoxide, and the second refractive layer is formed by depositing a second film material, the second film material includes magnesium fluoride.

7. The lens assembly according to claim 6, characterized in that: The number of the first refractive layer and the number of the second refractive layer are both multiple layers, and the first refractive layers and the second refractive layers are alternately stacked and distributed.

8. The lens assembly according to claim 7, characterized in that: The number of layers n1 of the first refractive layer satisfies, n1≥3; The number n2 of the second refractive layers satisfies n2≥3.

9. The lens assembly according to any one of claims 6 to 8, characterized in that: The first refractive layer further includes: aluminum oxide.

10. The lens assembly according to claim 9, characterized in that: The first refractive layer comprises titanium pentoxide, and the mass ratio of the titanium pentoxide to the aluminum oxide is 9:1; or The first refractive layer includes tantalum pentoxide, and the mass ratio of the tantalum pentoxide to the aluminum oxide is 9:1.