Three-dimensional structure conformal boron doping method and application thereof

By forming an interlaced thin film and alumina passivation layer on a three-dimensional structural substrate, combined with laser or rapid annealing technology, the shadow effect and structural damage problems of boron doping in three-dimensional structures are solved, and efficient and stable boron doping is achieved. , ensuring the stability and uniformity of the boron oxide film.

CN118943009APending Publication Date: 2024-11-12BEIJING SUPERSTRING ACAD OF MEMORY TECH +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411043105.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art has shadowing effects and structural damage problems in three-dimensional structural deposition, making it difficult to achieve conformal boron doping, and boron oxide films are easy to degrade in the environment. Thermal ALD method has difficulty in nucleation and film formation on the silicon surface. question.

Method used

By forming interlaced silicon oxide and boron oxide first laminated films on the surface of the silicon-based three-dimensional substrate, and interlaced aluminum oxide and boron oxide second laminated films, boron oxide impurities are passed through the auxiliary layer in combination with laser or rapid annealing technology. Advance to a silicon-based three-dimensional substrate, boron doping is achieved, and alumina passivation layer is covered on the second laminated film to protect the boron oxide.

Benefits of technology

The problems of shadowing effect and structural damage in plasma-enhanced ALD deposition are solved, and the damage-free boron doping is achieved, ensuring the stability and uniformity of the boron oxide film, and improving the control accuracy of doping concentration and film thickness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943009A_ABST
    Figure CN118943009A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of semiconductor preparation, in particular to a three-dimensional structure conformal boron doping method and application thereof, and the method comprises the following steps: removing an oxide layer on the surface of a silicon-based three-dimensional substrate; forming a first laminated film on the surface of the silicon-based three-dimensional substrate; forming a second laminated film on the surface of one side, far away from the silicon-based three-dimensional substrate, of the first laminated film; depositing an aluminum oxide passivation layer on the surface of one side, far away from the first laminated film, of the second laminated film; propelling boron impurities containing boron oxide into the silicon-based three-dimensional substrate through the auxiliary layer by using laser or rapid annealing so as to carry out boron doping on the silicon-based three-dimensional substrate; wherein the first laminated film comprises a silicon oxide layer and a boron oxide layer which are sequentially arranged in a staggered manner; and the second laminated film comprises an aluminum oxide layer and a boron oxide layer which are sequentially arranged in a staggered manner. The method not only solves the problem that the conformal deposition cannot be realized due to the shadow effect of the plasma enhanced ALD on the three-dimensional structure deposition, but also eliminates the problems of damage of the plasma to the device and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor preparation, and in particular to a three-dimensional structure conformal boron doping method and application thereof. Background Art

[0002] As device size continues to shrink, in order to improve the performance and integration of semiconductor devices, new device structures such as FinFET, nanowires and other three-dimensional (3D) structures are applied to the integrated circuit device manufacturing process. This three-dimensional structure poses great challenges to ultra-shallow silicon doping of traditional ion implantation, so it is necessary to study new methods to replace the traditional ion implantation doping process to solve the structural damage caused by ion implantation technology, the channel effect of implantation and the implantation shadow effect in the three-dimensional structure.

[0003] In order to overcome the limitations of traditional implantation, some new doping methods have been proposed. Among them, plasma doping cannot completely avoid damage-related problems, including transient enhanced diffusion (TED) during dopant activation; spin dopant (SOD) technology cannot be directly applied to three-dimensional structures; and single-layer doping and BBr3 gas phase doping face the problem of controlled deposition of dopant sources.

[0004] Atomic layer deposition technology has the characteristics of good conformality, uniformity, and atomic-scale thickness controllability because its growth mechanism is controlled by self-limiting surface reactions. ALD boron doping technology is expected to achieve uniform and conformal doping in three-dimensional nanoscale electronic devices.

[0005] At present, the existing technology mainly adopts plasma enhanced ALD deposition of B2O3 for doping (US011302527B2). However, on the one hand, since boron oxide is very easy to absorb moisture, when B2O3 is exposed to ambient air and contacts water vapor, it will be degraded due to the formation of volatile H3BO3. On the other hand, the thermal ALD method has the problem of difficult nucleation when depositing boron oxide on the silicon surface, and the film cannot be formed after a certain thickness.

[0006] Therefore, in the process of process development, it is necessary not only to screen suitable B source precursors and oxidants to solve the problem of controllable growth of the boron oxide film itself, but also to screen a suitable stable surface passivation layer so that in-situ deposition can protect B2O3 from damage, thereby achieving damage-free diffusion doping. In addition, due to the shadow effect of the plasma-enhanced ALD deposition method on the deposition of three-dimensional structures, conformal deposition cannot be achieved, and there are also problems such as plasma damage, which cannot meet the application requirements of the device well.

[0007] In view of this, the present invention is proposed. Summary of the invention

[0008] The purpose of the present invention is to provide a method for conformal boron doping of three-dimensional structures and its application, which not only solves the problem that the plasma enhanced atomic layer deposition method cannot achieve conformal deposition in three-dimensional structure deposition due to the shadow effect, but also solves the problem of structural damage caused by plasma.

[0009] In a first aspect, the present invention provides a method for conformal boron doping of a three-dimensional structure, comprising the following steps:

[0010] S1, removing the oxide layer on the surface of the silicon-based three-dimensional substrate;

[0011] S2, forming a first stacked thin film on the surface of the silicon-based three-dimensional substrate;

[0012] S3, forming a second stacked film on the surface of the first stacked film away from the silicon-based three-dimensional substrate;

[0013] S4, depositing an aluminum oxide passivation layer on the surface of the second stacked film away from the first stacked film;

[0014] S5. Using laser or rapid annealing to push boron impurities containing boron oxide through the auxiliary layer into the silicon-based three-dimensional substrate to perform boron doping on the silicon-based three-dimensional substrate;

[0015] The first stacked film is a silicon oxide layer and a boron oxide layer which are alternately arranged in sequence; and the second stacked film is an aluminum oxide layer and a boron oxide layer which are alternately arranged in sequence.

[0016] As a preferred embodiment of the present technical solution, step S1 includes: first, using the DHF method to remove the oxide layer on the silicon-based three-dimensional substrate, then placing the silicon-based three-dimensional substrate in the cavity of the atomic deposition equipment, evacuating the cavity, the cavity including the base, making the cavity base temperature 35-40°C, using a mixed gas of HF and NH3 to treat the silicon-based three-dimensional substrate for 20-40s, heating the temperature of the silicon-based three-dimensional substrate to 150-200°C, and baking in a hydrogen atmosphere for 40-80s to remove the surface oxide layer.

[0017] The ratio of hydrofluoric acid to water in DHF is 100:1. Due to its low concentration, its etching rate is very low, and it can initially etch the natural oxide film on the surface of the wafer.

[0018] The silicon-based three-dimensional substrate is further placed in the chamber of the atomic deposition equipment and evacuated. The chamber base temperature is 35-40°C, and the substrate is treated with a mixed gas of HF and NH3 for 20-40s. The wafer temperature is heated to 150-200°C and baked in a hydrogen atmosphere for 40-80 seconds to remove the natural oxide layer on the silicon surface of the wafer. At the same time, it has a very high selectivity for the silicon substrate and the SiN film. The wafer is then heated and baked to reduce impurities and defects on the wafer surface, improve the surface smoothness of the wafer, improve the conductivity of the wafer, reduce the concentration of impurities, and improve the electron mobility.

[0019] As a preferred embodiment of the present technical solution, step S2 includes: in the chamber of the atomic layer deposition equipment, alternately pulsing silicon-based compounds and boron-based compounds on the surface of the silicon-based three-dimensional substrate to form a first stacked film on the surface of the silicon-based three-dimensional substrate.

[0020] After removing the natural oxide on the surface of the silicon-based three-dimensional substrate, a first stacked film is further deposited on the surface of the silicon-based three-dimensional substrate to enable the nucleation and deposition of boron oxide on the wafer surface. The material of the first stacked film of the present invention includes silicon oxide and boron oxide. Using this as the first stacked film can effectively eliminate or slow down the diffusion of other metal ions in the subsequent oxide stacked film in the substrate, and reduce the doping concentration of other metal ions in the second stacked film in the silicon substrate.

[0021] Step S2 specifically includes:

[0022] First, the silicon-based three-dimensional substrate is vacuum-transferred to the chamber of the atomic layer deposition equipment, the chamber temperature is controlled to be 250-300°C, bis(diethylamino)silane is pulsed for 0.1-0.5s, vacuumed for 0.2-3s, then ozone is pulsed for 0.2-3s, and vacuumed for 0.2-3s; the process is repeated for 10-25 cycles to form a silicon oxide layer on the surface of the silicon-based three-dimensional substrate;

[0023] Then, in-situ pulsing trimethyl borate for 0.1-0.5s, vacuuming for 0.2-3s, pulsing ozone for 0.5-3s, and vacuuming for 0.2-3s; the treatment is repeated for 5-25 cycles to form a boron oxide layer on the surface of the silicon oxide layer away from the silicon-based three-dimensional substrate;

[0024] According to the requirements of the three-dimensional structure and doping, the preparation of the silicon oxide layer and the boron oxide layer is repeated to form a first stacked film. For example, the thickness of the first stacked film can be controlled to be 0.5-3 nm.

[0025] As a preferred embodiment of the present technical solution, step S3 includes: in the chamber of the atomic layer deposition equipment, alternately pulsing aluminum-based compounds and boron-based compounds on the surface of the first stacked film to form a second stacked film on the surface of the first stacked film away from the silicon-based three-dimensional substrate.

[0026] After forming a first stacked film on the surface of a silicon-based three-dimensional substrate, a second stacked film is further deposited on the surface of the first stacked film, which can well control the thickness of the doped oxide film and the boron content in the film. The material of the second stacked film of the present invention includes aluminum oxide and boron oxide. Using this as the second stacked film has the function of finely controlling the film thickness and the boron content in the film. By adjusting the thickness and concentration, the injection concentration effect can be accurately adjusted.

[0027] Step S3 specifically includes:

[0028] First, in a chamber of an atomic layer deposition device, the chamber temperature is controlled to be 80-150° C., trimethylaluminum is pulsed for 0.1-0.15 seconds, vacuum is applied for 0.2-3 seconds, ozone is pulsed for 0.2-3 seconds, and vacuum is applied for 0.2-3 seconds to form an aluminum oxide layer on the surface of the first stacked film;

[0029] Then, in-situ pulsing trimethyl borate for 0.1-0.5s, vacuuming for 0.2-3s, pulsing ozone for 0.5-3s, and vacuuming for 0.2-3s; the treatment is repeated for 10-20 cycles to form a boron oxide layer on the surface of the aluminum oxide layer away from the first stacked film;

[0030] According to the requirements of three-dimensional structure and doping, the preparation of aluminum oxide layer and boron oxide layer is repeated to form a second stacked film.

[0031] The present invention uses trimethyl borate as a boron source precursor and ozone as an oxidant when depositing a boron oxide layer, thereby effectively solving the problem that a thermal ALD method is difficult to form nuclei when depositing boron oxide on a silicon surface and that a film cannot be formed after a certain thickness.

[0032] In order to further protect the boron oxide layer from damage, the present invention further covers the surface of the boron oxide layer of the top layer of the second stacked film with an aluminum oxide passivation layer. The specific method is: in the chamber of the atomic layer deposition equipment, in-situ pulse trimethylaluminum for 0.1-0.15s, vacuum for 0.5-1.5s, pulse ozone for 0.5-1.5s, and vacuum for 1-3s; process for 3-5 cycles to obtain a stable passivation layer of a certain thickness.

[0033] As a preferred embodiment of the present technical solution, in step S5, when laser annealing is used, the wavelength range is 308nm-10.6um, and the energy density is 200mj / cm 2 -2j / cm 2 , annealing temperature is 900-1100℃, annealing time is 10ns-1ms;

[0034] When rapid annealing is used, the heating rate is greater than 250°C / s and the annealing time is 5-30s.

[0035] During laser annealing, a high-energy laser beam is used to rapidly irradiate the wafer. The wafer absorbs the laser energy and converts it into heat energy, causing the wafer to rapidly heat up locally to a high temperature, thereby allowing the boron atoms to diffuse in the crystal lattice and occupy replacement positions, achieving activation. Under the subsequent rapid cooling, the atoms in the crystal lattice are rearranged, thereby achieving the doping of the silicon substrate with boron impurities, achieving highly precise doping activation and defect repair.

[0036] After the boron impurities containing boron oxide are pushed through the auxiliary layer into the silicon substrate by laser or rapid annealing, the residual boron oxide and aluminum oxide film are further removed by hydrofluoric acid solution. The present invention does not strictly limit the concentration of the hydrofluoric acid solution, and a suitable concentration of hydrofluoric acid can be selected for etching as needed.

[0037] On the second aspect, the present invention also discloses the specific application of the above-mentioned three-dimensional structure conformal boron doping method in the ultra-shallow silicon doping preparation process of three-dimensional structure integrated circuit devices, which should also fall within the protection scope of the present invention.

[0038] The three-dimensional structure conformal boron doping method of the present invention has at least the following beneficial effects:

[0039] The present invention first forms a first stacked film and a second stacked film on the surface of a silicon-based three-dimensional substrate in sequence. The first stacked film has the ability to well eliminate or slow down the diffusion of other metal ions in the subsequent oxide stacked film in the substrate, reduce the doping concentration of other metal ions in the second stacked film in the silicon substrate, and the second stacked film can well control the thickness of the doped oxide film and the boron content in the film. Then, an aluminum oxide passivation layer is covered on the surface of the second stacked film, and finally, the boron impurities in the boron oxide are pushed into the silicon-based three-dimensional substrate through the auxiliary layer by laser or annealing to dope the silicon-based three-dimensional substrate, and finally realize boron doping on the three-dimensional structure. On the one hand, the method solves the problem of difficult nucleation and inability to form a film after a certain thickness of boron oxide by screening suitable boron source precursors and oxidants. On the other hand, aluminum oxide is selected as a passivation layer to protect the boron oxide film from damage, and then non-damage diffusion doping can be achieved during laser or rapid annealing. Therefore, the present invention not only solves the problem that the plasma enhanced atomic layer deposition method cannot achieve conformal deposition due to the shadow effect in the three-dimensional structure deposition, but also solves the problem of structural damage caused by plasma. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0041] Figure 1 This is a flow chart of the boron doping method for conformal three-dimensional structure of the present invention;

[0042] Figure 2 The first stacked film is formed on the surface of the silicon-based three-dimensional substrate of the present invention;

[0043] Figure 3 In the present invention, a second stacked film is formed on a surface of the first stacked film away from the silicon-based three-dimensional substrate;

[0044] Figure 4 In the present invention, the surface of the second stacked film away from the first stacked film is covered with an aluminum oxide passivation layer;

[0045] Figure 5 This is a graph showing the test results of B doping concentration in Example 1 of the present invention;

[0046] Figure 6 This is a graph showing the test results of B doping concentration in Comparative Example 1 of the present invention.

[0047] Reference numerals:

[0048] 1: first stacked film; 2: second stacked film; 3: aluminum oxide passivation layer. DETAILED DESCRIPTION

[0049] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0050] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form also includes the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this description, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0051] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0052] Example 1

[0053] S11, using a solution of hydrofluoric acid and water in a ratio of 100:1 to remove the oxide layer on the silicon-based three-dimensional substrate, then placing the silicon-based three-dimensional substrate in a chamber of an atomic deposition device, evacuating the chamber including a base, controlling the chamber base temperature to 35°C, using a mixed gas of HF and NH3 to treat the silicon-based three-dimensional substrate for 30s, heating the silicon-based three-dimensional substrate to 180°C and baking for 1min to remove the surface oxide layer;

[0054] S12, vacuum transfer the silicon-based three-dimensional substrate to the chamber of the atomic layer deposition equipment, control the chamber temperature to 270°C, pulse bis(diethylamino)silane 0.3 (source temperature 26°C), vacuum for 2s, then pulse ozone for 2s, and vacuum for 2s; process 15 cycles to form a silicon oxide layer on the surface of the silicon-based three-dimensional substrate;

[0055] In-situ pulse trimethyl borate for 0.3s (source temperature 21°C), vacuum for 2s, then pulse ozone for 2s, and vacuum for 2s; 20 cycles are performed to form a boron oxide layer on the surface of the silicon oxide layer away from the silicon-based three-dimensional substrate;

[0056] According to the requirements of the three-dimensional structure and doping, the silicon oxide layer and the boron oxide layer are repeatedly prepared to form a first stacked film ( Figure 2 );

[0057] S13, in a chamber of an atomic layer deposition device, controlling the chamber temperature to 100° C., pulsing trimethylaluminum for 0.12 s (source temperature 21° C.), vacuuming for 2 s, pulsing ozone for 2 s, and vacuuming for 2 s to form an aluminum oxide layer on the surface of the first stacked film;

[0058] In-situ pulse trimethyl borate for 0.3s (source temperature 21°C), vacuum for 2s, then pulse ozone for 2s, and vacuum for 2s; 15 cycles are performed to form a boron oxide layer on the surface of the aluminum oxide layer away from the first stacked film;

[0059] According to the requirements of the three-dimensional structure and doping, the aluminum oxide layer and the boron oxide layer are repeatedly prepared to form a second stacked film ( Figure 3 );

[0060] S14, in the chamber of the atomic layer deposition equipment, in-situ pulse trimethylaluminum for 0.125s (source temperature 21°C), vacuum for 1s, pulse ozone for 1s, vacuum for 2s; process for 4 cycles to form an aluminum oxide passivation layer ( Figure 4 );

[0061] S15, using laser annealing, and controlling the wavelength range to 308nm-10.6um, the energy density to 1j / cm 2, the annealing temperature is 1000° C., the annealing time is 500 ns, and the boron impurities containing boron oxide are pushed into the silicon-based three-dimensional substrate through the auxiliary layer to dope the silicon-based three-dimensional substrate;

[0062] S16. Use a hydrofluoric acid solution to remove the residual boron oxide and aluminum oxide films.

[0063] Example 2

[0064] S21. Use a solution of hydrofluoric acid and water in a ratio of 100:1 to remove the oxide layer on the silicon-based three-dimensional substrate. Then, place the silicon-based three-dimensional substrate in a chamber of an atomic deposition device and evacuate the chamber, wherein the chamber includes a base. The temperature of the chamber base is controlled to be 35°C. Use a mixed gas of HF and NH3 to treat the silicon-based three-dimensional substrate for 20 seconds. Heat the temperature of the silicon-based three-dimensional substrate to 200°C and bake for 40 seconds to remove the natural oxide layer on the surface.

[0065] S22, vacuum-transferring the silicon-based three-dimensional substrate to the chamber of the atomic layer deposition equipment, controlling the chamber temperature to 250° C., pulsing bis(diethylamino)silane for 0.5 s (source temperature 26° C.), vacuuming for 0.2 s, then pulsing ozone for 0.2 s, and vacuuming for 0.2 s; processing for 25 cycles to form a silicon oxide layer on the surface of the silicon-based three-dimensional substrate;

[0066] In-situ pulsing of trimethyl borate for 0.1 s (source temperature 21° C.), vacuuming for 0.2 s, then pulsing of ozone for 0.5 s, and vacuuming for 0.2 s; 25 cycles are performed to form a boron oxide layer on the surface of the silicon oxide layer away from the silicon-based three-dimensional substrate;

[0067] According to the requirements of the three-dimensional structure and doping, the silicon oxide layer and the boron oxide layer are repeatedly prepared to form a first stacked film;

[0068] S23, in a chamber of an atomic layer deposition device, controlling the chamber temperature to 80° C., pulsing trimethylaluminum for 0.15 s (source temperature 21° C.), vacuuming for 0.2 s, pulsing ozone for 0.2 s, and vacuuming for 0.2 s to form an aluminum oxide layer on the surface of the first stacked film;

[0069] In-situ pulse trimethyl borate for 0.1s (source temperature 21°C), vacuum for 0.2s, then pulse ozone for 0.5s, and vacuum for 0.2s; 20 cycles are performed to form a boron oxide layer on the surface of the aluminum oxide layer away from the first stacked film;

[0070] According to the requirements of the three-dimensional structure and doping, the aluminum oxide layer and the boron oxide layer are repeatedly prepared to form a second stacked film;

[0071] S24, in the chamber of the atomic layer deposition equipment, in-situ pulse trimethylaluminum for 0.15s (source temperature 21°C), vacuum for 0.5s, pulse ozone for 0.5s, and vacuum for 1s; process for 3 cycles to form an aluminum oxide passivation layer on the surface of the second stacked film away from the first stacked film;

[0072] S25, using laser annealing, and controlling the wavelength range to 308nm-10.6um, the energy density to 2j / cm 2 , the annealing temperature is 900° C., the annealing time is 1 ms, and the boron impurities containing boron oxide are pushed into the silicon-based three-dimensional substrate through the auxiliary layer to dope the silicon-based three-dimensional substrate;

[0073] S26. Use a hydrofluoric acid solution to remove the residual boron oxide and aluminum oxide films.

[0074] Example 3

[0075] S31. Use a solution of hydrofluoric acid and water in a ratio of 100:1 to remove the oxide layer on the silicon-based three-dimensional substrate. Then, place the silicon-based three-dimensional substrate in a chamber of an atomic deposition device and evacuate the chamber, wherein the chamber includes a base. Control the temperature of the chamber base to be 35° C., use a mixed gas of HF and NH3 to treat the silicon-based three-dimensional substrate for 40 seconds, heat the silicon-based three-dimensional substrate to 150° C. and bake for 80 seconds to remove the natural oxide layer on the surface.

[0076] S32, vacuum-transferring the silicon-based three-dimensional substrate to the chamber of the atomic layer deposition equipment, controlling the chamber temperature to 300° C., pulsing bis(diethylamino)silane for 0.1 s (source temperature 26° C.), evacuating for 3 s, then pulsing ozone for 3 s, and evacuating for 3 s; performing 10 cycles to form a silicon oxide layer on the surface of the silicon-based three-dimensional substrate;

[0077] In-situ pulse trimethyl borate for 0.5s (source temperature 21°C), vacuum for 3s, then pulse ozone for 3s, and vacuum for 3s; the process is repeated for 5 cycles to form a boron oxide layer on the surface of the silicon oxide layer away from the silicon-based three-dimensional substrate;

[0078] According to the requirements of the three-dimensional structure and doping, the silicon oxide layer and the boron oxide layer are repeatedly prepared to form a first stacked film;

[0079] S33, in a chamber of an atomic layer deposition device, controlling the chamber temperature to 150° C., pulsing trimethylaluminum for 0.1 s (source temperature 21° C.), vacuuming for 3 s, pulsing ozone for 3 s, and vacuuming for 3 s to form an aluminum oxide layer on the surface of the first stacked film;

[0080] In-situ pulse trimethyl borate for 0.5 s (source temperature 21° C.), vacuum for 3 s, then pulse ozone for 3 s, and vacuum for 3 s; the process is repeated for 15 cycles to form a boron oxide layer on the surface of the aluminum oxide layer away from the first stacked film;

[0081] According to the requirements of the three-dimensional structure and doping, the aluminum oxide layer and the boron oxide layer are repeatedly prepared to form a second stacked film;

[0082] S34, in the chamber of the atomic layer deposition equipment, in-situ pulse trimethylaluminum for 0.125s (source temperature 21°C), vacuum for 1s, pulse ozone for 1s, and vacuum for 2s; process 4 cycles to form an aluminum oxide passivation layer on the surface of the second stacked film away from the first stacked film;

[0083] S35, using rapid annealing, controlling the heating rate to 300° C. / s, and the annealing time to 20s, to push the boron impurities containing boron oxide through the auxiliary layer into the silicon-based three-dimensional substrate, so as to dope the silicon-based three-dimensional substrate;

[0084] S36. Use hydrofluoric acid solution to remove the residual boron oxide and aluminum oxide films.

[0085] Example 4

[0086] S41. Use a solution of hydrofluoric acid and water in a ratio of 100:1 to remove the oxide layer on the silicon-based three-dimensional substrate. Then, place the silicon-based three-dimensional substrate in a chamber of an atomic deposition device and evacuate the chamber, wherein the chamber includes a base. Control the temperature of the chamber base to be 35°C. Use a mixed gas of HF and NH3 to treat the silicon-based three-dimensional substrate for 30 seconds. Heat the temperature of the silicon-based three-dimensional substrate to 180°C and bake for 1 minute to remove the natural oxide layer on the surface.

[0087] S42, vacuum-transferring the silicon-based three-dimensional substrate to the chamber of the atomic layer deposition equipment, controlling the chamber temperature to 280° C., pulsing bis(diethylamino)silane for 0.4 s (source temperature 26° C.), evacuating for 1 s, then pulsing ozone for 2 s, and evacuating for 2 s; performing 20 cycles to form a silicon oxide layer on the surface of the silicon-based three-dimensional substrate;

[0088] In-situ pulse trimethyl borate for 0.2s (source temperature 21°C), vacuum for 1s, then pulse ozone for 2s, and vacuum for 2s; 15 cycles are performed to form a boron oxide layer on the surface of the silicon oxide layer away from the silicon-based three-dimensional substrate;

[0089] According to the requirements of the three-dimensional structure and doping, the silicon oxide layer and the boron oxide layer are repeatedly prepared to form a first stacked film;

[0090] S43, in a chamber of an atomic layer deposition device, controlling the chamber temperature to 120° C., pulsing trimethylaluminum for 0.1 s (source temperature 21° C.), vacuuming for 1 s, pulsing ozone for 1.5 s, and vacuuming for 2 s to form an aluminum oxide layer on the surface of the first stacked film;

[0091] In-situ pulse trimethyl borate for 0.3s (source temperature 21°C), vacuum for 2s, then pulse ozone for 2s, and vacuum for 2s; 15 cycles are performed to form a boron oxide layer on the surface of the aluminum oxide layer away from the first stacked film;

[0092] According to the requirements of the three-dimensional structure and doping, the aluminum oxide layer and the boron oxide layer are repeatedly prepared to form a second stacked film;

[0093] S44, in the chamber of the atomic layer deposition equipment, in-situ pulse trimethylaluminum for 0.15s (source temperature 21°C), vacuum for 1.5s, pulse ozone for 1.5s, and vacuum for 2s; process 4 cycles to form an aluminum oxide passivation layer on the surface of the second stacked film away from the first stacked film;

[0094] S45, using rapid annealing, controlling the heating rate to 300° C. / s, and the annealing time to 30s, to push the boron impurities containing boron oxide through the auxiliary layer into the silicon-based three-dimensional substrate, so as to dope the silicon-based three-dimensional substrate;

[0095] S46. Use hydrofluoric acid solution to remove the residual boron oxide and aluminum oxide films.

[0096] Comparative Example 1

[0097] S1. Use a solution of hydrofluoric acid and water in a ratio of 100:1 to remove the oxide layer on the silicon-based three-dimensional substrate. Then, place the silicon-based three-dimensional substrate in a chamber of an atomic deposition device and evacuate the chamber, including a base. Control the chamber base temperature to 35°C. Use a mixed gas of HF and NH3 to treat the silicon-based three-dimensional substrate for 30 seconds. Heat the silicon-based three-dimensional substrate to 180°C and bake for 1 minute to remove the surface oxide layer.

[0098] S2, vacuum-transferring the silicon-based three-dimensional substrate to the chamber of the atomic layer deposition equipment, controlling the chamber temperature to 120° C., pulsing trimethylaluminum for 0.3 s (source temperature 21° C.), evacuating for 2 s, pulsing ozone for 2 s, and evacuating for 2 s to form an aluminum oxide auxiliary layer on the surface of the silicon-based three-dimensional substrate;

[0099] S3. In the same chamber, in-situ pulse trimethyl borate for 0.3s (source temperature 21°C), vacuum for 2s, then pulse ozone for 2s, and vacuum for 2s; 15 cycles are performed to form a boron oxide film on the aluminum oxide auxiliary layer.

[0100] S4. In the same chamber, in-situ pulse trimethylaluminum for 0.125s (source temperature 21°C), vacuum for 1s, pulse ozone for 1s, vacuum for 2s; process 4 cycles to cover the surface of the boron oxide film with an aluminum oxide passivation layer;

[0101] S5. Using laser or rapid annealing to push boron impurities containing boron oxide through the auxiliary layer into the silicon substrate to dope the silicon-based three-dimensional substrate;

[0102] S6. Use hydrofluoric acid solution to remove the residual boron oxide and aluminum oxide films.

[0103] Figure 1 The figure is a flow chart of the method for conformal boron doping of three-dimensional structures of the present invention.

[0104] Table 1 shows the corresponding changes in process conditions and reaction data with increasing cycle times in Example 1 of the present invention.

[0105] Table 1

[0106]

[0107] The present invention measured the doping concentration of the three-dimensional structure doped with boron prepared in Example 1 and Comparative Example 1. The test results are as follows: Figure 5-6 shown.

[0108] Combined with Table 1 and Figure 5-6 It can be seen that the doping concentration of doping method B in Example 1 of the present invention can reach 8E+19, while the doping concentration of doping method B in comparative example 1 is 3E+19. It can be seen that the three-dimensional structure conformal boron doping method of the present invention is closer to the plasma enhanced ALD deposition B2O3 doping technology, and it can be seen from Table 1 that the present invention can also adjust the doping concentration according to the thickness of the second stacked film and effectively control the concentration of aluminum atoms in the silicon-based three-dimensional substrate.

[0109] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for conformal boron doping of a three-dimensional structure, characterized in that: The following steps are involved: S1, removing the oxide layer on the surface of the silicon-based three-dimensional substrate; S2, forming a first stacked thin film on the surface of the silicon-based three-dimensional substrate; S3, forming a second stacked film on the surface of the first stacked film away from the silicon-based three-dimensional substrate; S4, depositing an aluminum oxide passivation layer on the surface of the second stacked film away from the first stacked film; S5. Using laser or rapid annealing to push boron impurities containing boron oxide through the auxiliary layer into the silicon-based three-dimensional substrate to perform boron doping on the silicon-based three-dimensional substrate; The first stacked film is a silicon oxide layer and a boron oxide layer which are alternately arranged in sequence; and the second stacked film is an aluminum oxide layer and a boron oxide layer which are alternately arranged in sequence.

2. The method for conformal boron doping of a three-dimensional structure according to claim 1, characterized in that: Step S1 includes: using the DHF method to remove the oxide layer on the silicon-based three-dimensional substrate, then placing the silicon-based three-dimensional substrate in the chamber of the atomic deposition equipment, evacuating the chamber, controlling the temperature of the chamber base to 35-40°C, using a mixed gas of HF and NH3 to treat the silicon-based three-dimensional substrate for 20-40s, heating the temperature of the silicon-based three-dimensional substrate to 150-200°C, and baking in a hydrogen atmosphere for 40-80s to remove the surface oxide layer.

3. The method for conformal boron doping of a three-dimensional structure according to claim 1, characterized in that: Step S2 includes: in a chamber of an atomic layer deposition device, alternately pulsing a silicon-based compound and a boron-based compound on the surface of a silicon-based three-dimensional substrate to form a first stacked film on the surface of the silicon-based three-dimensional substrate.

4. The method for conformal boron doping of a three-dimensional structure according to claim 1, characterized in that: Step S3 includes: in the chamber of the atomic layer deposition equipment, alternately pulsing aluminum-based compounds and boron-based compounds on the surface of the first stacked film to form a second stacked film on the surface of the first stacked film away from the silicon-based three-dimensional substrate.

5. The method for conformal boron doping of a three-dimensional structure according to claim 3, characterized in that: In step S2, Vacuum transfer of the silicon-based three-dimensional substrate to the chamber of an atomic layer deposition device, control the chamber temperature to 250-300° C., pulse bis(diethylamino)silane for 0.1-0.5 s, vacuumize for 0.2-3 s, then pulse ozone for 0.2-3 s, and vacuumize for 0.2-3 s; perform 10-25 cycles to form a silicon oxide layer on the surface of the silicon-based three-dimensional substrate; In-situ pulsing trimethyl borate for 0.1-0.5s, vacuuming for 0.2-3s, then pulsing ozone for 0.5-3s, and vacuuming for 0.2-3s; processing for 5-25 cycles to form a boron oxide layer on the surface of the silicon oxide layer away from the silicon-based three-dimensional substrate; According to the requirements of three-dimensional structure and doping, the preparation of silicon oxide layer and boron oxide layer is repeated to form a first stacked film.

6. The method for conformal boron doping of a three-dimensional structure according to claim 4, characterized in that: In step S3, In a chamber of an atomic layer deposition device, the chamber temperature is controlled to be 80-150° C., trimethylaluminum is pulsed for 0.1-0.15 s, vacuuming for 0.2-3 s, ozone is pulsed for 0.2-3 s, and vacuuming for 0.2-3 s to form an aluminum oxide layer on the surface of the first stacked film; In-situ pulsing trimethyl borate for 0.1-0.5s, vacuuming for 0.2-3s, then pulsing ozone for 0.5-3s, and vacuuming for 0.2-3s; treating for 10-20 cycles to form a boron oxide layer on the surface of the aluminum oxide layer away from the first stacked film; According to the requirements of three-dimensional structure and doping, the preparation of aluminum oxide layer and boron oxide layer is repeated to form a second stacked film.

7. The method for conformal boron doping of a three-dimensional structure according to claim 1, characterized in that: Step S4 includes: in situ pulsing trimethylaluminum for 0.1-0.15s, vacuuming for 0.5-1.5s, pulsing ozone for 0.5-1.5s, and vacuuming for 1-3s in the chamber of the atomic layer deposition equipment; processing for 3-5 cycles to form an aluminum oxide passivation layer on the surface of the second stack film away from the first stack film.

8. The method for conformal boron doping of a three-dimensional structure according to claim 1, characterized in that: In step S5, when laser annealing is used, the wavelength range is 308nm-10.6um and the energy density is 200mj / cm 2 -2j / cm 2 , annealing temperature is 900-1100℃, annealing time is 10ns-1ms; When rapid annealing is used, the heating rate is greater than 250°C / s and the annealing time is 5-30s.

9. The method for conformal boron doping of a three-dimensional structure according to claim 1, characterized in that: The method further includes step S6 of removing the residual boron oxide and aluminum oxide films using a hydrofluoric acid solution.

10. Application of a method for conformal boron doping of a three-dimensional structure, characterized in that: The three-dimensional structure conformal boron doping method described in any one of claims 1 to 9 is applied in the ultra-shallow silicon doping preparation process of three-dimensional structure integrated circuit devices.

Citation Information

Cited By

  • Memory, and method for manufacturing memory