Method for reducing warping degree in wafer processing technology

By forming the first oxide layer and the top silicon nitride layer on the front of the wafer, and injecting nitrogen elements into the back surface before high-temperature oxidation to form the bottom silicon nitride layer, the warping problem caused by the LOCOS process is solved and the wafer is improved Flatness and stability enhance the reliability and production efficiency of the process.

CN118943074APending Publication Date: 2024-11-12THING ELEMENT SEMICON TECH (QINGDAO) CO LTD

Patent Information

Application Number
CN202410988695.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In semiconductor manufacturing, the deformation and stress of silicon wafers caused by the LOCOS process affect subsequent process steps and device performance, especially warping problems, are difficult to effectively solve.

Method used

By forming a first oxide layer on the front of the wafer, depositing the top silicon nitride layer, and performing high doses of ion implantation of nitrogen elements on the back of the wafer before high temperature oxidation, the bottom silicon nitride layer is formed to balance the second oxidation in the groove. The stress generated by the layer reduces the warpage.

Benefits of technology

It effectively reduces the warpage during wafer processing, improves the flatness and stability of the wafer, reduces processing errors and production losses, and enhances the reliability and repeatability of the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943074A_ABST
    Figure CN118943074A_ABST
Patent Text Reader

Abstract

The invention relates to a method for reducing the warping degree in a wafer processing technology, and the method comprises the following steps: carrying out the oxidation of the front surface of a wafer, and forming a first oxidation layer; depositing a top silicon nitride layer on the oxide layer on the front surface of the wafer through a chemical vapor deposition process; etching a groove in the front surface of the wafer; performing high-temperature oxidation on the wafer to form a second oxide layer in the groove; and before the wafer is subjected to high-temperature oxidation and the second oxide layer is formed in the groove, injecting nitrogen element into the back surface of the wafer through a high-dose ion injection method, so that a bottom silicon nitride layer is formed on the back surface of the wafer when the wafer is subjected to high-temperature oxidation. According to the invention, the technical problem of warping degree in the wafer processing process is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of semiconductor technology, and in particular relates to a method for reducing warpage in a wafer processing process. Background Art

[0002] In the field of semiconductor manufacturing, device isolation technology is a key process to ensure that the components in an integrated circuit are electrically insulated from each other. Traditional device isolation methods have many challenges, such as complex manufacturing processes and potential impact on device performance. As a classic device isolation technology, the LOCOS (selective oxidation of silicon) process is widely used in the manufacture of semiconductor devices due to its effective isolation performance and high manufacturing maturity.

[0003] The LOCOS process uses the principle of silicon selective oxidation to achieve silicon selective oxidation in deep grooves (groove depth greater than 0.5 microns) under the protection of a silicon nitride mask. Grooves are created on the silicon nitride layer through photolithography and etching processes to form a LOCOS structure in the grooved area.

[0004] The core advantage of the LOCOS process lies in its simple and efficient isolation effect. By utilizing the electrical insulation properties of SiO2, the LOCOS process can form reliable electrical isolation between devices while reducing interference between adjacent devices. However, the LOCOS process also faces some challenges. For example, the stress that may be introduced during the deposition of silicon nitride and the growth of the LOCOS process can cause the silicon wafer to warp, affecting subsequent process steps and device performance. Summary of the invention

[0005] In view of the deficiencies existing in the related art, the present invention provides a method for reducing warpage in a wafer processing process to solve the warpage problem in the wafer processing process.

[0006] In a possible implementation, a method for reducing warpage in a wafer processing process is provided, comprising the following steps: oxidizing the front side of the wafer to form a first oxide layer (SiO 2 ); depositing a top silicon nitride layer on the oxide layer on the front side of the wafer by a chemical vapor deposition process; etching a groove on the front side of the wafer; performing high-temperature oxidation on the wafer to form a second oxide layer (LOCOS) in the groove; and also including: before performing high-temperature oxidation on the wafer to form the second oxide layer in the groove, implanting nitrogen into the back side of the wafer by a high-dose ion implantation method; so that when the wafer is subjected to high-temperature oxidation, a bottom silicon nitride layer is formed on the back side of the wafer.

[0007] In one possible implementation, nitrogen is implanted on the back of the wafer by high-dose ion implantation, with an implantation dose greater than 1E16 / cm 2 .

[0008] In a possible implementation manner, high temperature oxidation is performed on the wafer at a temperature of 1100° C.

[0009] In a possible implementation, after a groove is etched on the front side of the wafer, nitrogen is implanted into the back side of the wafer by a high-dose ion implantation method.

[0010] In one possible implementation, the top silicon nitride layer is deposited by phase chemical vapor deposition (PECVD) at a temperature of 400° C., a total gas pressure of 2-3 Torr, and a deposition power of 1 kW.

[0011] In one possible implementation, the thickness of the top silicon nitride layer is 1000 Å-2000 Å.

[0012] In a possible implementation manner, the nitrogen element is implanted into the back side of the wafer repeatedly for 2 to 3 times.

[0013] Based on the above technical scheme, the method for reducing warpage in the wafer processing process of the present invention forms a first oxide layer by oxidizing the front side of the wafer, deposits a top silicon nitride layer thereon, then etches a groove and performs high-temperature oxidation, and injects nitrogen into the back side of the wafer before high-temperature oxidation, so that during high-temperature oxidation, a second oxide layer is formed in the groove while a bottom silicon nitride layer is formed on the back side, thereby avoiding the growth of oxide on the back side, balancing the stress generated when the second oxide layer is formed in the groove, and improving the warping problem during wafer processing. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0015] Figure 1 A schematic flow chart of a method for reducing warpage in a wafer processing process according to an embodiment;

[0016] Figure 2 This is a comparison diagram of improvements in processing wafers according to the method for reducing warpage in the wafer processing process of the present application.

[0017] In the figure:

[0018] 1. First oxide layer; 2. Top silicon nitride layer; 3. Groove; 4. Second oxide layer; 5. Bottom silicon nitride layer; 51. Nitrogen element; 6. Wafer. DETAILED DESCRIPTION

[0019] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0020] In the description of the present invention, it should be understood that the terms "center", "lateral", "longitudinal", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0021] The terms "first", "second", and "third" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the technical features indicated. Thus, a feature defined as "first", "second", and "third" may explicitly or implicitly include one or more of the features.

[0022] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0023] In order to solve the problem of warping during wafer processing, the present application provides a method for reducing warping in a wafer processing process.

[0024] See also Figure 1 According to the first aspect of the present application, a method for reducing warpage in a wafer processing process comprises the following steps: oxidizing the front side of the wafer to form a first oxide layer 1;

[0025] On the first oxide layer 1 on the front side of the wafer 6, a top silicon nitride layer 2 is deposited by a chemical vapor deposition process;

[0026] Etching a groove 3 on the front side of the wafer;

[0027] The wafer is subjected to high temperature oxidation to form a second oxide layer 4 in the groove;

[0028] Before the wafer is subjected to high temperature oxidation to form the second oxide layer 4 in the groove, nitrogen element 51 is implanted into the back of the wafer by high dose ion implantation so that a bottom silicon nitride layer 5 is formed on the back of the wafer when the wafer is subjected to high temperature oxidation.

[0029] In the above scheme, see Figure 1 , in the order of (1), (2), (3), (4), (5) and (6), first, the front side of the wafer is oxidized to form the first oxide layer 1 in (2) to relieve the stress caused by the subsequent deposition of Nitride, i.e., the top silicon nitride layer; then, the top silicon nitride layer 2 in (3) is deposited on the first oxide layer 1 on the front side by a chemical vapor deposition process, and the top silicon nitride layer provides mechanical stress to offset the subsequent processing stress; after etching the groove 3 on the front side of the wafer, a second oxide layer 5 is formed in the groove by high-temperature oxidation. At this time, in order to balance the stress in the front groove 3 during the oxidation process, before the high-temperature oxidation (6), a high-dose ion implantation of nitrogen element is performed on the back side of the wafer, i.e., the nitrogen element 51 in (5). During the high-temperature oxidation process, the implanted nitrogen element forms the bottom silicon nitride layer 5, which balances the stress generated by the second oxide layer 4 in the groove 3 and reduces the warpage.

[0030] The above method reduces the warpage of the wafer during processing. By depositing silicon nitride layers on the front and back of the wafer, the stress in all directions is balanced, so that the wafer remains flat after high-temperature processing. The high-dose ion implantation of nitrogen ensures the uniformity and thickness of the silicon nitride layer, further enhancing the reliability and repeatability of the process.

[0031] In one possible embodiment, the method for reducing the warpage in the wafer processing process includes implanting nitrogen into the back side of the wafer by high-dose ion implantation, wherein the implantation dose is greater than 1E16 / cm 2 .

[0032] By injecting a high dose of nitrogen into the back of the wafer, a uniform and dense bottom silicon nitride layer is formed during the high-temperature oxidation process. This layer of silicon nitride can effectively balance the mechanical stress on the front of the wafer and reduce the warpage.

[0033] Injection greater than 1E16 / cm 2 The high dose of nitrogen ensures that the formed silicon nitride layer has sufficient thickness and strength, thereby effectively balancing the stress of the wafer during processing. This method improves the flatness and stability of the wafer and reduces processing errors and production losses caused by warpage.

[0034] In a possible implementation manner, high temperature oxidation is performed on the wafer at a temperature of 1100° C.

[0035] Oxidation treatment at a high temperature of 1100°C helps to form a uniform oxide layer on the surface of the wafer, while promoting the diffusion of nitrogen on the back of the wafer and the formation of a silicon nitride layer. Heat treatment during high-temperature oxidation can effectively reduce the internal stress of the wafer, thereby reducing warpage.

[0036] Oxidation treatment at high temperature improves the quality and uniformity of the oxide layer, helps to form a dense oxide layer and silicon nitride layer, and effectively reduces the warpage. This method enhances the mechanical strength and thermal stability of the wafer, making it suitable for subsequent complex processing.

[0037] In a possible implementation, after a groove is etched on the front side of the wafer, nitrogen is implanted into the back side of the wafer by a high-dose ion implantation method.

[0038] The step of injecting nitrogen into the back side of the wafer can be completed before high temperature oxidation. As an implementation method, nitrogen is injected into the back side after etching the grooves on the front side to ensure that the nitrogen diffuses evenly during the high temperature oxidation process and forms a bottom silicon nitride layer. This operation step helps to form a synchronous stress balance on the front and back sides, further reducing the warpage.

[0039] By injecting nitrogen on the back side after etching the grooves on the front side, the synchronization of the formation of the silicon nitride layer and the oxidation process of the grooves is ensured, thereby more effectively balancing the internal stress of the wafer, further reducing the warpage, and enhancing the mechanical stability and processing accuracy of the wafer.

[0040] In one possible implementation, the top silicon nitride layer 2 is deposited by phase chemical vapor deposition (PECVD) at a temperature of 400° C., a total gas pressure of 2-3 Torr, and a deposition power of 1 kW.

[0041] By controlling the temperature, gas pressure and deposition power in the PECVD process, the thickness and uniformity of the top silicon nitride layer 2 can be precisely controlled. This method ensures that the top silicon nitride layer 2 forms a dense protective layer on the wafer surface, providing a mask for the subsequent etching grooves 3, and providing the necessary mechanical stress for the subsequent high-temperature oxidation to reduce the warpage.

[0042] The top silicon nitride layer 2 is deposited under the above process conditions by a chemical vapor deposition (PECVD) process, thereby ensuring the quality and performance of the top silicon nitride layer and effectively reducing the warpage of the wafer.

[0043] In one possible implementation, the thickness of the top silicon nitride layer is 1000 Å-2000 Å.

[0044] Controlling the thickness of the top silicon nitride layer within the range of 1000A-2000A can provide sufficient mechanical stress to balance the stress of the wafer without affecting subsequent process steps. The silicon nitride layer within this thickness range can effectively reduce the warpage of the wafer.

[0045] In a possible implementation manner, the nitrogen element is implanted into the back side of the wafer repeatedly for 2 to 3 times.

[0046] By repeatedly injecting nitrogen, a uniform and dense silicon nitride layer can be formed on the back of the wafer. Multiple injections can enhance the diffusion and deposition of nitrogen on the back of the wafer, thereby further reducing the warpage.

[0047] In a possible implementation manner, the depth d of the high-dose nitrogen element implanted is directly proportional to the depth D of the trench.

[0048] In the above scheme, the deeper the trench depth, the greater the stress generated by depositing the second oxide layer. Therefore, a relatively thick bottom silicon nitride layer is required to prevent the formation of SiO on the back of the wafer. 2 , thereby balancing the stress caused by LOCOS growth and reducing the warpage of the wafer.

[0049] As one implementation method, for example, the groove depth D is 0.5um, and the depth d of the injected nitrogen element is 100nm; after the injection is completed, after high-temperature oxidation at 1100°C, the second oxide layer and the bottom silicon nitride layer are formed, and the bottom silicon nitride layer balances the stress during the formation of the second oxide layer and reduces the warping of the wafer.

[0050] In the above solution, the depth d of the implanted nitrogen element and the depth D of the trench satisfy the following relationship: d≥0.2D.

[0051] In the above solution, the depth of the nitrogen implantation can also be determined according to the production process requirements, while satisfying d=100nm-150nm.

[0052] As a method for reducing warpage in a wafer processing process according to an embodiment of the present invention, the specific description is as follows:

[0053] The LOCOS (selective oxidation of silicon) process is a device isolation technology that uses silicon nitride as a mask to achieve selective oxidation of silicon in deep trenches (groove depth greater than 0.5um).

[0054] First, a layer of oxide is grown around the groove to relieve the stress caused by the deposition of Nitride. Then a layer of Nitride is deposited and a groove is dug at the corresponding position to generate oxide in the groove to form LOCOS. 2 The electrical insulation properties of the two devices are isolated from each other.

[0055] The presence of the top silicon nitride layer / Nitride can not only effectively block the growth of the second oxide layer 4 / thermal oxide during high-temperature oxidation in the groove, but also improve the problem of excessive curling / warpage caused by LOCOS. Silicon nitride / Nitride can be deposited using a furnace tube process, which can be deposited on both the front and back sides of the wafer, and can effectively alleviate the warpage after LOCOS growth, but the process is time-consuming, which is not conducive to improving chip production efficiency, and the related furnace tubes will cause defects / defects. Therefore, here as a preferred implementation of the Nitride process, LPCVD machine and high-dose ion implantation Implant machine are used to deposit and grow silicon nitride / Nitride, and the top silicon nitride layer / Nitride is directly deposited on the front side of the wafer using a low-pressure chemical vapor deposition (LPCVD) process, and a high-dose N element is implanted into the back side of the wafer, which can shorten the process time and reduce the impact of particles on product yield. It can also solve the problem of excessive wafer warpage after growing LOCOS.

[0056] Using the process of chemical vapor deposition + high-dose ion implantation, after the first oxide layer 1 is grown by high-temperature oxidation / thermal oxidation, a top silicon nitride layer 2 / Nitride of 1000A~2000A is deposited on the front of the wafer using chemical vapor deposition at 400℃, 2~3Torr, and 1kW power. Then a groove 3 is etched and a second oxide layer 4, namely LOCOS, is grown in the groove. In order to avoid the warpage being too large after the growth of LOCOS, it is necessary to deposit a layer of Nitride on the back as well. Here, ion implantation is used, using a High Current Implant machine, to implant (repeatedly implant) a high dose of 1E16 or more N elements into the back of the wafer. During the heating process of the LOCOS process at the target process temperature of 1100℃, the N element reacts with the surrounding Si atoms to generate Si 3 N 4 , which can effectively block the generation of back oxide, thereby improving the problem of wafer warpage being too large.

[0057] Before the oxide layer in the groove, i.e. LOCOS growth, a high-dose N element is injected using a high-dose implanter, so that it reacts with the Si substrate during the heating stage of the LOCOS process to form a silicon nitride layer / Nitride.

[0058] Compared with the prior art, the method for reducing warpage in the wafer processing technology of the present invention has the following beneficial effects:

[0059] Compared with the method of furnace tube Nitride deposition, the combination of PECVD and high-dose ion implanter can effectively solve the warpage problem caused by the LOCOS process, solve the particle problem caused by furnace tube Nitride deposition, and shorten the overall process time. It is helpful to improve chip production efficiency and increase revenue, reduce particle interference, and improve product quality and yield.

[0060] See also Figure 2 The traditional LOCOS growth method is to use furnace tubes to deposit nitride Nitride as a mask for local oxidation LOCOS growth of silicon to solve the problem of excessive warpage caused by the LOCOS process. Because the furnace tubes used are low-pressure tubes and the deposition process is more likely to cause excessive particles.

[0061] / The problem of high particle size. The present invention does not use a furnace to deposit nitride / Nitride, but uses a PECVD+Implant / injection combination method. Nitride is deposited on the front side of the wafer using plasma chemical vapor deposition PECVD, and nitrogen is injected into the back side using Implant. The nitrogen then reacts with Si to generate Nitride during the LOCOS process. This novel process solution can solve both the problem of excessive warpage caused by the LOCOS process and the problem of high particles. In the chip manufacturing process, too many particles will damage the device structure of a single chip unit / die, thereby affecting the yield of the wafer. The invention solves this major problem.

[0062] Finally, it should be noted that: the various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0063] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention is described in detail with reference to the preferred embodiments, ordinary technicians in the field should understand that the specific implementation methods of the present invention can still be modified or some technical features can be replaced by equivalents without departing from the spirit of the technical solution of the present invention, which should be included in the scope of the technical solution for protection of the present invention.

Claims

1. A method for reducing warpage in a wafer processing process, It is characterized in that The following steps are involved: The front side of the wafer is oxidized to form the first oxide layer (SiO 2 ); Depositing a top silicon nitride layer on the first oxide layer on the front side of the wafer by a chemical vapor deposition process; Etching grooves on the front side of the wafer; The wafer is subjected to high temperature oxidation to form a second oxide layer (LOCOS) in the groove; It also includes: before performing high-temperature oxidation on the wafer to form a second oxide layer in the groove, injecting nitrogen into the back side of the wafer by high-dose ion implantation; so that when the wafer is subjected to high-temperature oxidation, a bottom silicon nitride layer is formed on the back side of the wafer.

2. The method for reducing warpage in a wafer processing process according to claim 1, It is characterized in that Nitrogen is implanted on the back of the wafer by high-dose ion implantation, with an implantation dose greater than 1E16 / cm 2 .

3. The method for reducing warpage in a wafer processing process according to claim 2, It is characterized in that The wafer is subjected to high temperature oxidation at a temperature of 1100°C.

4. The method for reducing warpage in a wafer processing process according to claim 3, It is characterized in that After etching grooves on the front side of the wafer, nitrogen is implanted into the back side of the wafer using high-dose ion implantation.

5. The method for reducing warpage in a wafer processing process according to claim 4, It is characterized in that The top silicon nitride layer was deposited by phase chemical vapor deposition (PECVD) at a temperature of 400° C., a total gas pressure of 2-3 Torr, and a deposition power of 1 kW.

6. The method for reducing warpage in a wafer processing process according to claim 5, It is characterized in that The thickness of the top silicon nitride layer is 1000A-2000A.

7. The method for reducing warpage in a wafer processing process according to claim 6, It is characterized in that The nitrogen injection into the back side of the wafer is repeated 2 to 3 times.

Citation Information

Patent Citations

  • Method for preparing local silicon oxidation isolation structure

    CN101350327A

  • Method for preparing back electrical insulation isolation region of IBC battery by ion implantation technology, IBC battery and preparation method of IBC battery

    CN118016767A

  • Semiconductor wafer and manufacture thereof

    JP1996227834A

  • Shallow trench isolation in semiconductor device

    KR1020050069200A

  • Method for eliminating wafer warpage and composite substrate

    WO2019128524A1

Cited By

  • Method for improving alignment of contact hole and groove in insulated gate bipolar transistor

    CN121487280A