Graphene-based chip electromagnetic shielding structure
By using graphene films to absorb electromagnetic waves in radio frequency equipment, the chip is susceptible to interference and cavity self-excitation is solved, efficient electromagnetic shielding is achieved, cost and complexity is reduced, and it is suitable for high-density integrated application scenarios.
Patent Information
- Application Number
- CN202411007252.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
AI Technical Summary
In miniaturized high-density integrated radio frequency equipment, the chip's operating frequency is the same as the resonant frequency of the cavity, which will cause self-excitation, which will affect the working life of the chip. The traditional shielded metal cavity structure design is complex and costly.
The film made of graphene material is fixed on the inner wall of the shielded cavity through vapor deposition and wet transfer coating technology. The high electromagnetic wave absorption characteristics and two-dimensional planar structure characteristics of graphene are used to weaken the resonant strength of the cavity. , avoid self-excitation.
It effectively reduces the resonance strength of the electromagnetic shielding structure, avoids the occurrence of chip self-excitation, improves the reliability of the chip, and is simple in design and low in cost. It is suitable for application scenarios in complex electromagnetic environments.
Smart Images

Figure CN118943125A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electromagnetic shielding, and in particular to a graphene-based chip electromagnetic shielding structure. Background Art
[0002] As the size of the current RF front end becomes smaller and smaller, and the integration becomes higher and higher, the electromagnetic interference environment faced by the equipment becomes more and more complex. Therefore, the demand for electromagnetic shielding in RF equipment, integrated circuits, SIP, etc. is also increasing. Shielded metal cavity is currently a commonly used electromagnetic shielding structure, but the shielding characteristics of the traditional shielded metal cavity are very dependent on the structural design, and its inherent resonance characteristics are also strongly related to the structural design. Under the premise of miniaturization and high-density integration, the structural design becomes extremely difficult. When the operating frequency of the chip is the same as the resonance frequency of the cavity, self-excitation will occur. The self-excitation phenomenon will affect the working life of the chip, and in severe cases, it will even damage the chip. Therefore, the occurrence of self-excitation should be avoided as much as possible. Summary of the invention
[0003] In view of the problem in the prior art that the chip generates self-excitation due to the operating frequency being the same as the resonance frequency of the cavity, the present invention provides a chip electromagnetic shielding structure based on graphene.
[0004] The present invention is achieved through the following technical solutions:
[0005] A graphene-based chip electromagnetic shielding structure comprises a cover plate, a tube shell and a chip. The tube shell is an upper opening structure, the chip is fixed inside the tube shell, the cover plate is arranged at the opening of the tube shell, the cover plate comprises a cover plate base and a film, and the film is arranged on the lower surface of the cover plate base facing the inside of the tube shell; the film is made of graphene material, the square resistance of the film is 100-500Ω / Sq, and the thickness of the film is less than 10μm.
[0006] Preferably, a boss is provided below the base, and the lower surface of the boss has the same size as the inner side of the tube shell; a film is provided on the lower surface of the boss, and the size of the film is the same as the size of the lower surface of the boss.
[0007] Preferably, the thin film is grown and prepared by a vapor deposition method, and is coated on the boss by a wet transfer method.
[0008] Preferably, the growth process of the thin film includes a temperature rise stage, a temperature holding stage, a two-step deposition growth stage and a temperature drop stage;
[0009] In the heating stage, the raw materials are heated to 1000-1050° C. in a mixed atmosphere of hydrogen and argon;
[0010] During the heat preservation stage, the atmosphere is maintained and the annealing is completed by heat preservation for 20 minutes;
[0011] The two-step deposition growth stage includes a nucleation stage and a growth stage. In the nucleation stage, the mixture of hydrogen and methane is kept warm for 10 to 15 minutes; in the growth stage, the mixture of hydrogen and methane is kept warm for 5 to 10 minutes.
[0012] During the cooling stage, the furnace was cooled down to 100°C in an argon atmosphere by a combination of furnace cooling and air cooling, and then the furnace was opened to cool naturally to room temperature.
[0013] Preferably, in the nucleation stage, the flow rate of hydrogen is 500-1000 sccm, and the flow rate of methane is 10-20 sccm.
[0014] Preferably, during the growth stage, the flow rate of hydrogen is 50-100 sccm, and the flow rate of methane is 100-200 sccm.
[0015] Preferably, polymethyl methacrylate is used as the transfer medium for wet transfer.
[0016] Preferably, the process of wet transfer film is as follows:
[0017] Step 1, coating a transfer medium on the surface of the film;
[0018] Step 2, corroding and cleaning the film;
[0019] Step 3, placing the cleaned film on a transfer medium, removing the transfer medium after drying and cleaning until the film is fixed on the cover plate.
[0020] Preferably, the corrosion of the sample includes pre-corrosion and continuous corrosion. The pre-corrosion liquid used in the pre-corrosion is: during the continuous corrosion, firstly in FeCl 3 The steel is immersed in the solution and then continuously corroded in a dilute hydrochloric acid solution.
[0021] Preferably, the tube shell is made of iron-nickel alloy material.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The present invention is a chip electromagnetic shielding structure based on graphene. The high electromagnetic wave absorption characteristics and two-dimensional planar structural characteristics of graphene are utilized. The graphene film can effectively absorb electromagnetic waves in the cavity, greatly weaken the resonance intensity of the electromagnetic shielding structure, and avoid the self-excitation phenomenon, thereby achieving the effect of protecting the chip. The present invention has the characteristics of simple design, convenient application, and low cost. It is particularly suitable for application scenarios such as integrated circuits / chips with complex electromagnetic environments and high electromagnetic shielding requirements, and has high practical value and economic benefits.
[0024] Furthermore, it is pasted / coated on the inner wall of the shielding cavity in the form of coating. Compared with the traditional closed metal cavity shielding structure, it can greatly reduce the self-excited Q value of the shielding cavity without affecting the original structural size and performance of the cavity, prevent the occurrence of chip self-excitation, and improve chip reliability. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic diagram of a graphene-based chip electromagnetic shielding structure of the present invention;
[0026] Figure 2 It is a side view of a tube shell in a graphene-based chip electromagnetic shielding structure of the present invention;
[0027] Figure 3 It is a top view of a tube shell in a graphene-based chip electromagnetic shielding structure of the present invention;
[0028] Figure 4 It is a side view of a cover plate in a graphene-based chip electromagnetic shielding structure of the present invention;
[0029] Figure 5 It is a top view of a cover plate in a graphene-based chip electromagnetic shielding structure of the present invention;
[0030] Figure 6 is the shielding cavity reflection coefficient (without printed graphene)
[0031] Figure 7 This is the reflection coefficient of the shielding cavity of the present invention (printed with graphene).
[0032] In the figure, 1. cover plate base; 2. film; 3. tube shell base; 4. side wall. DETAILED DESCRIPTION
[0033] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.
[0034] The present invention discloses a chip electromagnetic shielding structure based on graphene, referring to Figure 1 , including a cover plate, a tube shell and a chip, the tube shell is an upper opening structure, and the tube shell in this embodiment is made of iron-nickel alloy, referring to Figure 2 , 3 , including a connected shell base 3 and a square annular side wall 4. The shell base 3 is a cubic structure with a size of 14*14mm and a thickness of 3.3mm. On the shell base 3 is a side wall 44. The side wall 4 is a square annular design. The outer square side length is 9.5mm*9.5mm, which is the same size as the cover base 1; the inner square side length is 8.5mm*8.5mm. The height of the side wall 4 is 1.8mm and the thickness of the side wall 4 is 0.5mm. Figure 38*8 metal vias are opened on the shell base 3, and the chip inside the electromagnetic shielding structure can be connected to the external circuit through the metal vias. The shell has the characteristics of light weight, small size, simple production, and does not affect the electrical characteristics of the chip itself.
[0035] The chip is fixed inside the tube shell, and the cover plate is set at the opening of the tube shell. Figure 4 , 5 The cover plate includes a cover plate base 1 and a film 2, and the film 2 is arranged on the lower surface of the cover plate base 1 facing the inside of the tube shell. A boss is arranged below the cover plate base 1, and the lower surface of the boss has the same size as the inner side of the tube shell; the film 2 is arranged on the lower surface of the boss, and the size of the film 2 is the same as the size of the lower surface of the boss. In this embodiment, the shape of the cover plate base 1 is a square, the size is 9.5mm*9.5mm, the overall height is 100um, the material is iron-nickel alloy, and there is an arc transition at the four corners to prevent scratches during processing. The cover plate base 1 has a downward square raised area with a size of 8.5mm*8.5mm, and the size of the square protrusion corresponds to the size of the tube shell cavity.
[0036] The square resistance of the film 2 is 100-500Ω / Sq. The square resistance of the film 2 has a certain relationship with the frequency of the absorbed electromagnetic wave. Since the frequency range of the electromagnetic wave is 20-40GHz, in this embodiment, a layer of graphene film 2 with a square resistance of 400Ω / sq is applied on the surface of the square protrusion. The shape of the graphene film 2 is consistent with the shape of the protruding part of the cover base 1, and the thickness is less than 10um. The graphene film 2 can effectively absorb electromagnetic waves in the cavity, greatly weaken the resonance intensity of the electromagnetic shielding structure, and avoid the self-excitation phenomenon, thereby achieving the effect of protecting the chip.
[0037] The film 2 is made of graphene material, the square resistance of the film 2 is 400Ω / sq, and the thickness of the film 2 is less than 10μm. The film 2 is grown and prepared by vapor deposition, and is coated on the boss by wet transfer. Graphene has the characteristics of low cost, simple preparation, and convenient operation, and can be applied to various application scenarios such as compact structure and small size.
[0038] The growth process of the film 2 includes a heating stage, a heat preservation stage, a two-step deposition growth stage, and a cooling stage, as follows:
[0039] In the heating stage, the raw materials are heated to 1000-1050°C in a mixed atmosphere of hydrogen and argon while ventilating and exhausting;
[0040] During the heat preservation stage, the atmosphere is maintained and the annealing is completed by heat preservation for 20 minutes;
[0041] The two-step deposition growth stage includes a nucleation stage and a growth stage. In the nucleation stage, the temperature is kept in a mixed atmosphere of hydrogen and methane for 10 to 15 minutes, the flow rate of hydrogen is 500 to 1000 sccm, and the flow rate of methane is 10 to 20 sccm; in the growth stage, the flow rate of hydrogen is 50 to 100 sccm, the flow rate of methane is 100 to 200 sccm, and the temperature is kept in a mixed atmosphere of hydrogen and methane for 5 to 10 minutes;
[0042] During the cooling stage, the temperature is lowered to 100° C. by furnace cooling combined with air cooling while ventilating and exhausting in an argon atmosphere, and then the argon is turned off, and the temperature is naturally lowered to room temperature by opening the furnace to obtain a graphene film 2. The graphene film 2 has a two-dimensional planar structure and high electromagnetic wave absorption characteristics, which can effectively solve the inherent resonance characteristic problem of the shielding cavity.
[0043] During wet transfer, polymethyl methacrylate is used as the transfer medium for transfer. The process is as follows:
[0044] Step 1, coating a transfer medium on the surface of the film 2;
[0045] Step 2, etching and cleaning of film 2; the etching of film 2 includes pre-etching and continuous etching, and the pre-etching solution used in pre-etching is a mixed solution of water, dilute hydrochloric acid and hydrogen peroxide; in continuous etching, it is first immersed in FeCl3 solution, and then continuously etched in dilute hydrochloric acid solution.
[0046] Pre-corrosion: The film 2 is immersed in the pre-corrosion solution for 25-30 minutes to remove the surface oxide. The volume fraction of water: dilute hydrochloric acid: hydrogen peroxide is 20:1:1.
[0047] Continuous corrosion: The film 2 is immersed in a 15% FeCl3 solution for 2 to 3 hours to corrode most of the metal copper foil. Too long a time will damage the graphene film 2. Then take it out and place it in a dilute hydrochloric acid solution (the volume ratio of water to dilute hydrochloric acid is 50:1) to continue etching for 20 minutes to remove the remaining metal residues.
[0048] Cleaning: Take out the sample and clean it three times with plasma water, each time for 20 minutes.
[0049] Step 3, placing the cleaned sample on the cover plate, and after natural drying for 12 hours, removing the transfer medium with acetone solvent, and finally transferring the graphene film 2 from the copper foil to the cover plate.
[0050] In the electromagnetic simulation software HFSS, the electromagnetic shielding structure with graphene film and the electromagnetic shielding structure without graphene film are modeled respectively, and the quality factor Q value of the three main resonance modes of the two structures is compared by using the eigenmode simulation (the eigenmode simulation can directly obtain the resonance intensity parameter Q value of the structure) (the larger the Q value, the stronger the resonance and the more likely it is to occur self-excitation; the smaller the Q value, the weaker the resonance and the less likely it is to occur self-excitation). The simulation results of the quality factor are shown in the table:
[0051]
[0052]
[0053]
[0054] From the results, it can be seen that the resonant frequencies of the three resonance modes without graphene film are 23.8277GHz, 35.6277GHz, and 39.6218GHz, and the corresponding Q values of the three resonance modes are 1604.65, 1944.71, and 1999.57, respectively. The resonant frequencies of the three resonance modes with graphene film are 23.7788GHz, 38.8830GHz, and 43.6382GHz, and the corresponding Q values of the three resonance modes are 0.98, 1.61, and 1.86, respectively. It was found that the frequency of the resonance mode shifted after the introduction of graphene film, indicating that after the introduction of graphene film, the electromagnetic shielding structure changed and a perturbation phenomenon occurred; the quality factor Q value was greatly reduced, which verified the characteristics of graphene film in reducing resonance and preventing self-excitation.
[0055] In order to further verify the effect of using graphene materials in the cavity to suppress the cavity self-resonance, we processed the actual object for testing. The method for measuring the cavity Q value adopts the single probe electrical coupling test method. The Q value calculation formula is as follows:
[0056]
[0057]
[0058] Among them, Q L is the cavity loaded Q value, f 0 is the resonant frequency, BW 3dB is 3dB bandwidth.
[0059] The measured reflection coefficient of the metal shielding cavity without printed graphene is as follows Figure 6 As shown, it can be clearly observed that at a frequency of 24.73 GHz, the shielding cavity produces a resonance point, and the reflection coefficient reaches -12 dB, which is harmful to the shielding cavity and may cause self-excitation of the electronic devices inside the shielding cavity.
[0060] The reflection coefficient of the metal shielding cavity of printed graphene is as above Figure 7 As shown, it can be observed that at the frequency of 24.73 GHz, the reflection coefficient is only -3 dB, and the resonance of the shielding cavity is significantly suppressed.
[0061] The present invention utilizes the high electromagnetic wave absorption characteristics of graphene materials to solve the problem that the chip is susceptible to external interference and prevents the chip itself from affecting the external electromagnetic environment; at the same time, the two-dimensional planar structure characteristics and high electromagnetic wave absorption characteristics of graphene are utilized to solve the problem of self-excitation caused by the inherent resonance characteristics of the traditional electromagnetic shielding cavity structure, thereby affecting / damaging the chip; and provides a chip electromagnetic shielding solution with low cost, good effect, easy operation and wide application range.
[0062] The above description is only a preferred embodiment of the present invention and is not intended to impose any limitation on the technical solution of the present invention. Those skilled in the art should understand that, without departing from the spirit and principles of the present invention, the technical solution can also be subjected to several simple modifications and substitutions, and these modifications and substitutions are also within the scope of protection covered by the claims.
Claims
1. A graphene-based chip electromagnetic shielding structure, characterized in that: The invention comprises a cover plate, a tube shell and a chip. The tube shell is an upper opening structure. The chip is fixed inside the tube shell. The cover plate is arranged at the opening of the tube shell. The cover plate comprises a cover plate base (1) and a film (2). The film (2) is arranged on the lower surface of the cover plate base (1) facing the inside of the tube shell. The film (2) is made of graphene material. The square resistance of the film (2) is 100 to 500 Ω / Sq. The thickness of the film (2) is less than 10 μm.
2. The graphene-based chip electromagnetic shielding structure according to claim 1, characterized in that: A boss is arranged below the cover base (1), and the lower surface of the boss has the same size as the inner side of the tube shell; a film (2) is arranged on the lower surface of the boss, and the size of the film (2) is the same as the size of the lower surface of the boss.
3. The graphene-based chip electromagnetic shielding structure according to claim 2, characterized in that: The film (2) is grown and prepared by a vapor deposition method and is coated on the boss by wet transfer.
4. The graphene-based chip electromagnetic shielding structure according to claim 3, characterized in that: The growth process of the thin film (2) includes a heating stage, a heat preservation stage, a two-step deposition growth stage and a cooling stage; In the heating stage, the raw materials are heated to 1000-1050° C. in a mixed atmosphere of hydrogen and argon; During the heat preservation stage, the atmosphere is maintained and the annealing is completed by heat preservation for 20 minutes; The two-step deposition growth stage includes a nucleation stage and a growth stage. In the nucleation stage, the mixture of hydrogen and methane is kept warm for 10 to 15 minutes; in the growth stage, the mixture of hydrogen and methane is kept warm for 5 to 10 minutes. During the cooling stage, the furnace was cooled down to 100°C in an argon atmosphere by a combination of furnace cooling and air cooling, and then the furnace was opened to cool naturally to room temperature.
5. The graphene-based chip electromagnetic shielding structure according to claim 4, characterized in that: In the nucleation stage, the flow rate of hydrogen is 500-1000 sccm, and the flow rate of methane is 10-20 sccm.
6. The graphene-based chip electromagnetic shielding structure according to claim 4, characterized in that: During the growth phase, the flow rate of hydrogen is 50-100 sccm, and the flow rate of methane is 100-200 sccm.
7. The graphene-based chip electromagnetic shielding structure according to claim 3, characterized in that: During wet transfer, polymethyl methacrylate is used as the transfer medium.
8. The graphene-based chip electromagnetic shielding structure according to claim 1, characterized in that: The process of wet transfer film (2) is as follows: Step 1, coating a transfer medium on the surface of the film (2); Step 2, etching and cleaning the film (2); Step 3, placing the cleaned film (2) on a transfer medium, removing the transfer medium after drying and cleaning, until the film (2) is fixed on the cover plate.
9. The graphene-based chip electromagnetic shielding structure according to claim 8, characterized in that: The corrosion of the samples includes pre-corrosion and continuous corrosion. The pre-corrosion liquid used in the pre-corrosion is a mixed solution of water, dilute hydrochloric acid and hydrogen peroxide; in the continuous corrosion, the samples are first immersed in a FeCl3 solution and then continuously corroded in a dilute hydrochloric acid solution.
10. The graphene-based chip electromagnetic shielding structure according to claim 1, characterized in that: The tube shell is made of iron-nickel alloy material.