Silicon carbide-based H-type gate power device and preparation method thereof

By designing the H-type polysilicon gate and corresponding preparation methods in silicon carbide-based MOSFET devices, the problem of gate oxide degradation in the device in high temperature and high pressure environment is solved, and the device performance is improved.

CN118943189APending Publication Date: 2024-11-12HATCHIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410997054.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The gate oxide layer reliability issues of silicon carbide-based MOSFET devices, especially the time-dependent dielectric breakdown and bias temperature instability effects, lead to the degradation of the device's performance in high temperature and high pressure environments.

Method used

Design a silicon carbide-based H-type gate power device, adopting the H-type polysilicon gate and corresponding preparation method, by setting an oxide layer and a top metal layer at the cross-section of the polysilicon gate, and forming a passivation layer on the gate oxide layer to reduce The area of ​​the polysilicon gate is to reduce the gate capacitance.

Benefits of technology

Effectively release large voltage stress, avoid gate oxide layer degradation, and reduce the area of ​​polysilicon gate, thereby improving device performance and improving device withstand voltage and operating frequency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943189A_ABST
    Figure CN118943189A_ABST
Patent Text Reader

Abstract

The invention relates to the field of semiconductor devices, and discloses a silicon carbide-based H-type gate power device and a preparation method thereof. The device comprises a back drain metal layer, an n + type silicon carbide substrate and an n type drift layer which are sequentially stacked from bottom to top, two sides of the top of the n-type drift layer are respectively provided with a p-type base region; a p +-type source region and an n +-type source region are wrapped in the p-type base region; a first source metal layer, an oxide layer and a second source metal layer are sequentially arranged above the n-type drift layer from left to right, a polysilicon gate is wrapped in the oxide layer, a gate oxide layer adjacent to the polysilicon gate is arranged below the oxide layer, and the cross section of the polysilicon gate is H-shaped; a top metal layer is arranged above the first source electrode metal layer, the oxide layer and the second source electrode metal layer, and a passivation layer is arranged above the top metal layer. By means of the mode, large voltage stress can be released, and degradation of the gate oxide layer is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor devices, and in particular to a silicon carbide-based H-type gate power device and a preparation method thereof. Background Art

[0002] Silicon carbide (SiC) is a typical representative of the third generation of semiconductors. Silicon carbide materials have a wide bandgap, high breakdown voltage, high thermal conductivity, high electron saturation rate and other advantages. Therefore, power electronic devices made of silicon carbide materials have higher voltage resistance, current confidentiality and operating frequency. They can work in high frequency and high temperature environments, have high reliability, and are suitable for harsh working environments. Therefore, silicon carbide materials as third generation power electronic devices have become the most important development direction of power electronic technology, and have important application prospects in military and civil fields.

[0003] Metal Oxide Semiconductor Field Effect Transistor (MOSFET) is a voltage-controlled device with the advantages of fast switching speed, good high-frequency performance, low noise, and low driving power. It is a commonly used power switching device. Compared with silicon-based MOSFETs of the same level, silicon carbide-based MOSFETs have the advantages of higher voltage resistance and higher operating temperature due to their material properties. Without the need to introduce complex structural design, they can achieve lower specific on-resistance than silicon-based materials under the same voltage conditions. It is expected to become the most suitable power switching device working under high temperature and high pressure conditions. However, the reliability issues of silicon carbide-based MOSFET devices have also restricted their commercial development and widespread application.

[0004] However, the reliability of silicon carbide-based MOSFET devices, especially the reliability of the gate oxide layer, including the TDDB (Time Dependent Dielectric Breakdown) effect and BTI (Bias Temperature Instability) effect of the gate oxide layer, has restricted the further application and development of the device. Because silicon carbide has a large number of interface state defects in Si / SiO2, under high voltage stress, electrons in SiC can easily pass through the barrier and enter the gate oxide, resulting in severe degradation of the gate oxide layer, affecting the performance of power devices. Summary of the invention

[0005] The present invention provides a silicon carbide-based H-type gate power device and a preparation method thereof, which can release large voltage stress and avoid degradation of a gate oxide layer.

[0006] In order to solve the above technical problems, a technical solution adopted by the present invention is: to provide a silicon carbide-based H-type gate power device, comprising: a back drain metal layer, an n+ type silicon carbide substrate, and an n-type drift layer stacked in sequence from bottom to top; p-type base regions are respectively arranged on both sides of the top of the n-type drift layer, a p+ type source region and an n+ type source region are wrapped in the p-type base region, the p+ type source region and the n+ type source region are arranged side by side and contact each other on the side, and the p+ type source region is arranged close to the side of the n-type drift layer; a first source metal layer, an oxide layer and a second source metal layer are arranged in sequence from left to right above the n-type drift layer, a polysilicon gate is wrapped in the oxide layer, a gate oxide layer adjacent to the polysilicon gate is arranged below the oxide layer, and the cross-section of the polysilicon gate is H-shaped; a top metal layer is arranged above the first source metal layer, the oxide layer and the second source metal layer, and a passivation layer is arranged above the top metal layer.

[0007] According to one embodiment of the present invention, the depth of the p-type base region is 1.5 μm, and the doping concentration is 1e17 cm -3 ~1e18 cm -3 The depth of the n+ type source region is 0.2 μm, and the doping concentration is greater than 1e19 cm -3 The depth of the p+ source region is 3.0 μm and the doping concentration is 1e18 cm -3 ~1e19 cm -3 .

[0008] According to an embodiment of the present invention, the thickness of the gate oxide layer is 500 Å.

[0009] According to an embodiment of the present invention, the thickness of the polysilicon gate is 4000A.

[0010] According to an embodiment of the present invention, the thickness of the oxide layer is 1.0 μm.

[0011] According to one embodiment of the present invention, the passivation layer includes a plasma enhanced tetraethyl orthosilicate layer with a thickness of 6000 Å, a plasma enhanced silicon nitride layer with a thickness of 300 Å, and a polyimide film layer with a thickness of 7 μm.

[0012] According to an embodiment of the present invention, the thickness of the first source metal layer and the second source metal layer are both 1000 Å.

[0013] According to an embodiment of the present invention, the thickness of the top metal layer is 4 μm.

[0014] According to one embodiment of the present invention, the back drain metal layer includes a metal titanium layer with a thickness of 1000A, a metal nickel layer with a thickness of 2000A, and a metal silver layer with a thickness of 10kA.

[0015] In order to solve the above technical problems, another technical solution adopted by the present invention is: to provide a method for preparing the silicon carbide-based H-type gate power device, comprising:

[0016] Step S1: epitaxially growing an n-type drift layer on an n+ silicon carbide substrate;

[0017] Step S2: forming a p-type base region on the n-type drift layer by sequentially growing a first masking layer process, a high temperature oxidation process, a photolithography process, an etching process, and an ion implantation process;

[0018] Step S3: using the first masking layer to grow a layer of low-pressure tetraethoxy silicate glass, and forming an n+ type source region through a plasma dry isotropic etching process, a self-alignment process and an ion implantation process;

[0019] Step S4: removing the first masking layer by wet method, re-depositing the second masking layers of each layer, and forming a p+ type source region by photolithography, etching and ion implantation;

[0020] Step S5: growing a gate oxide layer through a carbon film growth and high temperature activation process and a nitrogen annealing process;

[0021] Step S6: depositing saturated doped polysilicon on the gate oxide layer, and forming a polysilicon gate through photolithography and etching processes, wherein the cross section of the polysilicon gate is H-shaped;

[0022] Step S7: depositing a layer of borophosphosilicate glass on the polysilicon gate and the gate oxide layer, and forming an oxide layer through photolithography and etching processes;

[0023] Step S8: forming a first source metal layer and a second source metal layer on both sides of the oxide layer by a metal deposition process and a rapid annealing process;

[0024] Step S9: forming a top metal layer through a sputtering process and an etching process, and depositing a passivation layer on the top metal layer;

[0025] Step S10: forming a back drain metal layer on the back of the n+ type silicon carbide substrate by a metal deposition process and a laser annealing process, thereby completing the preparation of a silicon carbide-based H-type gate power device.

[0026] The beneficial effects of the present invention are as follows: by setting an H-type polysilicon gate, not only can the large voltage stress be released and the degradation of the gate oxide layer be avoided, but also the area of ​​the polysilicon gate can be reduced, the gate capacitance can be reduced, and thus the performance of the device can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1It is a schematic cross-sectional structure diagram of a silicon carbide-based H-type gate power device according to an embodiment of the present invention;

[0028] Figure 2 is another cross-sectional structural schematic diagram of a silicon carbide-based H-type gate power device according to an embodiment of the present invention;

[0029] Figure 3 It is a schematic flow chart of a method for preparing a silicon carbide-based H-type gate power device according to an embodiment of the present invention;

[0030] Figure 4 Schematic diagram of the structure formed in step S1 of the method for preparing a silicon carbide-based H-type gate power device according to an embodiment of the present invention;

[0031] Figure 5 Schematic diagram of the structure formed in step S2 of the method for preparing a silicon carbide-based H-type gate power device according to an embodiment of the present invention;

[0032] Figure 6 Schematic diagram of the structure formed in step S3 of the method for preparing a silicon carbide-based H-type gate power device according to an embodiment of the present invention;

[0033] Figure 7 is a schematic diagram of a structure formed in step S4 in the method for preparing a silicon carbide-based H-type gate power device according to an embodiment of the present invention;

[0034] Figure 8 is a schematic diagram of a structure formed in step S5 in the method for preparing a silicon carbide-based H-type gate power device according to an embodiment of the present invention;

[0035] Fig. 9 is a schematic diagram of a structure formed in step S5 in the method for preparing a silicon carbide-based H-type gate power device according to an embodiment of the present invention;

[0036] Fig.10 Schematic diagram of the structure formed in step S6 of the method for preparing a silicon carbide-based H-type gate power device according to an embodiment of the present invention;

[0037] Fig.11 yes Fig.10 Schematic diagram of the cross-section structure along the AA line;

[0038] Fig.12 yes Fig.10 Schematic diagram of the cross-sectional structure along the BB line;

[0039] Fig.13 is a schematic diagram of a structure formed in step S7 in the method for preparing a silicon carbide-based H-type gate power device according to an embodiment of the present invention;

[0040] Fig.14 is a schematic diagram of a structure formed in step S8 in the method for preparing a silicon carbide-based H-type gate power device according to an embodiment of the present invention;

[0041] Fig.15 is a schematic diagram of a structure formed in step S9 in the method for preparing a silicon carbide-based H-type gate power device according to an embodiment of the present invention;

[0042] Fig.16 is a schematic diagram of a structure formed in step S9 in the method for preparing a silicon carbide-based H-type gate power device according to an embodiment of the present invention;

[0043] Fig.17 It is a schematic diagram of the structure formed in step S10 in the method for preparing a silicon carbide-based H-type gate power device according to an embodiment of the present invention.

[0044] The meanings of the symbols in the accompanying drawings are:

[0045] 1-back drain metal layer; 2-n+ type silicon carbide substrate; 3-n type drift layer; 4-p type base region; 5-p+ type source region; 6-n+ type source region; 7-first source metal layer; 8-oxide layer; 9-second source metal layer; 10-gate oxide layer; 11-polysilicon gate; 12-top metal layer; 13-passivation layer; 14-first masking layer; 15-second masking layer; 16-carbon film. DETAILED DESCRIPTION

[0046] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0047] The terms "first", "second" and "third" in the present invention are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. Thus, the features defined as "first", "second" and "third" can explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. All directional indications (such as up, down, left, right, front, back...) in the embodiments of the present invention are only used to explain the relative position relationship, movement, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication also changes accordingly. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not limited to the listed steps or units, but optionally also includes steps or units that are not listed, or optionally also includes other steps or units inherent to these processes, methods, products or devices.

[0048] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present invention. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0049] Figure 1 , Figure 2 Schematic diagram of the structure of a silicon carbide-based H-type gate power device at different cross-section positions according to an embodiment of the present invention. Figure 1 and Figure 2 The silicon carbide-based H-type gate power device comprises a back drain metal layer 1, an n+-type silicon carbide substrate 2, and an n-type drift layer 3 which are stacked in sequence from bottom to top; p-type base regions 4 are respectively arranged on both sides of the top of the n-type drift layer 3, and a p+-type source region 5 and an n+-type source region 6 are wrapped in the p-type base region 4. The p+-type source region 5 and the n+-type source region 6 are arranged side by side and contact each other on the side, and the p+-type source region 5 is arranged close to the side of the n-type drift layer 3; a first source metal layer 7, an oxide layer 8, and a second source metal layer 9 are arranged in sequence from left to right above the n-type drift layer 3, a polysilicon gate 11 is wrapped in the oxide layer 8, and a gate oxide layer 10 adjacent to the polysilicon gate 11 is arranged below the oxide layer 8, and the cross section of the polysilicon gate 11 is H-shaped; a top metal layer 12 is arranged above the first source metal layer 7, the oxide layer 8, and the second source metal layer 9, and a passivation layer 13 is arranged above the top metal layer 12.

[0050] The silicon carbide-based H-type gate power device of the embodiment of the present invention can not only release the large voltage stress and avoid the degradation of the gate oxide layer 10 by setting the H-type polysilicon gate 11, but also reduce the area of ​​the polysilicon gate 11 and reduce the gate capacitance, thereby improving the performance of the device.

[0051] As an embodiment, the thickness of the n+ type silicon carbide substrate 2 is 350 μm, and the doping concentration is greater than 1e19 cm -3 .

[0052] As an embodiment, the thickness of the n-type drift layer 3 is 9.5 μm to 10.5 μm, and the doping concentration is 1e15 cm -3 ~1e16 cm -3 .

[0053] As an embodiment, the depth of the p-type base region 4 is 1.5 μm, and the doping concentration is 1e17 cm -3 ~1e18 cm -3 ; The depth of the n+ source region 6 is 0.2 μm, and the doping concentration is greater than 1e19 cm -3 ; The depth of the p+ source region 5 is 3.0 μm, and the doping concentration is 1e18 cm -3 ~1e19 cm -3 .

[0054] As an embodiment, the thickness of the gate oxide layer 10 is 500 Å.

[0055] As an embodiment, the thickness of the polysilicon gate 11 is 4000 Å.

[0056] As an embodiment, the thickness of the oxide layer 8 is 1.0 μm.

[0057] As an embodiment, the passivation layer 13 includes a plasma enhanced tetraethyl orthosilicate layer with a thickness of 6000 Å, a plasma enhanced silicon nitride layer with a thickness of 300 Å, and a polyimide film layer with a thickness of 7 μm.

[0058] As an embodiment, the thickness of the first source metal layer 7 and the second source metal layer 9 are both 1000 Å.

[0059] As an embodiment, the thickness of the top metal layer 12 is 4 μm.

[0060] As an embodiment, the back drain metal layer 1 includes a metal titanium layer with a thickness of 1000A, a metal nickel layer with a thickness of 2000A, and a metal silver layer with a thickness of 10kA.

[0061] Figure 3FIG. 1 is a flow chart of a method for preparing a silicon carbide-based H-type gate power device according to an embodiment of the present invention. It should be noted that if substantially the same results are achieved, the method of the present invention is not limited to Figure 3 The process sequence shown is limited. Figure 3 As shown, the method comprises the steps of:

[0062] Step S1: epitaxially growing an n-type drift layer on an n+ silicon carbide substrate.

[0063] In step S1, Figure 4 As shown, the thickness of the n+ type silicon carbide substrate 2 is 350 μm, and the doping concentration is greater than 1e19 cm -3 The thickness of the n-type drift layer 3 is 9.5 μm to 10.5 μm, and the doping concentration is 1e15 cm -3 ~1e16 cm -3 .

[0064] Step S2: forming a p-type base region on the n-type drift layer by sequentially performing a first masking layer growth process, a high temperature oxidation process, a photolithography process, an etching process, and an ion implantation process.

[0065] In step S2, first, a first masking layer 14 is grown on the cleaned n-type drift layer 3. The first masking layer 14 is a sandwich structure, including a thermal oxide layer with a thickness of 500A, a transition layer with a thickness of 1000A, and a low-pressure tetraethoxy silicate glass layer with a thickness of 2μm, which are arranged from bottom to top. Among them, the thermal oxide layer is used as a shielding layer during injection, which can effectively avoid injection channel tunneling; the transition layer can connect the thermal oxide layer and the low-pressure tetraethoxy silicate glass layer, and the endpoint detection signal is strong during etching. Then, after high-temperature densification, photolithography patterning, photoresist coating, exposure and development are carried out. The thickness of the photoresist is 2μm, the side wall is smooth, and the side wall angle is greater than 88±2°. Next, the etching process is carried out. The etching is carried out using an ICP (Inductive Coupled Plasma) or TCP (Transformer Coupled Plasma) dry etching machine with better anisotropy. First, the top low-pressure tetraethoxysilicate glass layer is etched for 2μm, and the end point is stopped at the transition layer. After the over-etching is completed, the etching is switched to the transition layer, and the end point is stopped at the thermal oxide layer. Finally, the photoresist is removed and cleaned to prepare for ion implantation. Aluminum is injected at high energy at a high temperature of 500°C. The injection is divided into multiple times. Generally, 3 to 5 injections are required, and the injection angle is 0°. For example, taking 5 injections as an example, the energy of the first injection is 30kev, and the dose is 5e15 cm -2 The second implantation energy is 100keV and the dose is 5e13 cm -2The third injection energy is 250kev and the dose is 5e13cm -2 The fourth injection energy is 350kev and the dose is 5e14 cm -2 The fifth injection energy is 500kev and the dose is 5e15cm -2 , forming a depth of about 1.5 μm and a doping concentration of 1e17 cm -3 ~1e18cm -3 The p-type base region 4, such as Figure 5 shown.

[0066] Step S3: using the first masking layer to grow a layer of low-pressure tetraethoxy silicate glass, and forming an n+ type source region through a plasma dry isotropic etching process, a self-alignment process and an ion implantation process.

[0067] In step S3, a low-pressure tetraethoxy silicate glass with a thickness of about 5 kA is grown using the first masking layer 14, and a 0.5 μm conductive channel is formed by plasma dry isotropic etching and self-alignment process. Then, nitrogen is injected at a high temperature of 500°C, and the injection is performed in multiple times, generally 3 to 5 times, with an injection angle of 0°. For example, taking 4 injections as an example, the first injection energy is 20 kev and the dose is 5e14 cm -2 The second implantation energy is 40keV and the dose is 5e14 cm -2 The third injection energy is 60keV and the dose is 5e14 cm -2 The fourth injection energy is 100keV and the dose is 8e13 cm -2 , with a depth of 0.2 μm and a doping concentration greater than 1e19 cm -3 The n+ type source region 6, such as Figure 6 shown.

[0068] Step S4: removing the first masking layer by wet method, re-depositing the second masking layer of each layer, and forming a p+ type source region by photolithography, etching and ion implantation.

[0069] In step S4, the first masking layer 14 is removed by wet method, and the second masking layer 15 of each layer is re-deposited, and photolithography patterning, photoresist coating, exposure and development are performed in sequence, and the second masking layer is etched, and P-type ion implantation is performed after the photoresist is removed. Aluminum is implanted at high energy at a high temperature of 500°C, and the implantation is performed in multiple times. Generally, 4 to 7 implantations are required, and the implantation angle is 0°. For example, taking 7 implantations as an example, the first implantation energy is 30kev and the dose is 5e15cm -2 The second implantation energy is 100keV and the dose is 5e14 cm -2The third implantation energy is 250kev and the dose is 5e14 cm -2 The fourth injection energy is 350kev and the dose is 5e14 cm -2 The fifth injection energy is 500kev and the dose is 5e15cm -2 The sixth injection energy is 600kev and the dose is 5e14 cm -2 The seventh injection energy is 700kev and the dose is 5e13 cm -2 , forming a depth of about 3.0 μm and a doping concentration of 1e18 cm -3 ~1e19 cm -3 The p+ type source region 5, such as Figure 7 shown.

[0070] Step S5: growing a gate oxide layer through a carbon film growth and high temperature activation process and a nitrogen annealing process.

[0071] In step S5, a carbon film 16 is sputtered in a metal sputtering chamber, and then activated in a high temperature furnace at 1650° C. for 30 min, and finally the carbon film 16 is removed by sulfuric acid. Figure 8 Before growing the gate oxide layer 10, a nitrogen annealing process is added, and the gas used in the nitrogen annealing process is NO / O 2 Specifically, the sample surface was treated with a gas containing 2% NO for 1 hour before thermal oxidation, and then 2 The sample was thermally oxidized in a gas with a NO content of 5% to grow a gate oxide layer 10 with a thickness of 500 Å. Finally, the sample was thermally annealed in a gas with a NO content of 2% for 1 hour. The temperature was controlled at 1250°C throughout the process. Fig. 9 The gate oxide layer 10 is shown.

[0072] Step S6: depositing saturated doped polysilicon on the gate oxide layer, and forming a polysilicon gate through photolithography and etching processes, wherein the cross section of the polysilicon gate is H-shaped.

[0073] In step S6, firstly, saturated doped polysilicon with a thickness of about 4000A is deposited in a low temperature furnace tube, and the polysilicon is made into an H-type by photolithography and etching to form a polysilicon gate 11. Figure 10-12 shown.

[0074] Step S7: depositing a layer of borophosphosilicate glass on the polysilicon gate and the gate oxide layer, and forming an oxide layer through photolithography and etching processes.

[0075] In step S7, a layer of borophosphosilicate glass with a thickness of 1 μm is first deposited as a dielectric isolation layer, a pattern is exposed using a photomask of an ohmic contact hole, and then the borophosphosilicate glass is dry-etched as an ohmic contact hole to form an oxide layer 8, as shown in FIG. Fig.13 shown.

[0076] Step S8: forming a first source metal layer and a second source metal layer on both sides of the oxide layer by a metal deposition process and a rapid annealing process.

[0077] In step S8, a nickel metal layer with a thickness of 1000A is deposited on both sides of the oxide layer 8, and a rapid annealing is performed at 500°C to 700°C for 60 seconds to form a layer of Ni x Si y The alloy layer is removed by etching solution. 2 The nickel without alloy layer is finally rapidly annealed at 980℃ for 60 seconds to make Ni x Si y The alloy layer becomes a high temperature alloy to form a good ohmic contact, that is, the first source metal layer 7 and the second source metal layer 9, such as Fig.14 shown.

[0078] Step S9: forming a top metal layer through a sputtering process and an etching process, and depositing a passivation layer on the top metal layer.

[0079] In step S9, a layer of titanium aluminum metal with a thickness of 4 μm is sputtered on the first source metal layer 7, the oxide layer 8 and the second source metal layer 9, and the gate and the source are isolated by metal etching to form a top metal layer 12, such as Fig.15 A passivation layer 13 is deposited on the top metal layer 12, as shown. Fig.16 The passivation layer 13 includes a plasma enhanced tetraethyl orthosilicate layer with a thickness of 6000 Å, a plasma enhanced silicon nitride layer with a thickness of 300 Å, and a polyimide film layer with a thickness of 7 μm.

[0080] Step S10: forming a back drain metal layer on the back of the n+ type silicon carbide substrate by a metal deposition process and a laser annealing process, thereby completing the preparation of the silicon carbide-based H-type gate power device.

[0081] In step S10, a blue film is attached to the front side of the n+ type silicon carbide substrate 2, and the back side is thinned to 100 μm. Then, the blue film is removed, cleaned, titanium is evaporated on the back side, and an ohmic contact is made by laser annealing to form a back drain metal layer 1, thereby completing the preparation of the silicon carbide-based H-type gate power device. Fig.17 As shown, the back drain metal layer 1 includes a metal titanium layer with a thickness of 1000A, a metal nickel layer with a thickness of 2000A, and a metal silver layer with a thickness of 10kA.

[0082] The method for preparing a silicon carbide-based H-type gate power device in an embodiment of the present invention can not only release large voltage stress and avoid degradation of the gate oxide layer 10 by preparing an H-type polysilicon gate 11, but also reduce the area of ​​the polysilicon gate 11 and reduce the gate capacitance, thereby improving the performance of the device.

[0083] The above are only implementation modes of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A silicon carbide-based H-gate power device, characterized in that: It comprises a back drain metal layer, an n+ type silicon carbide substrate and an n-type drift layer which are stacked in sequence from bottom to top; p-type base regions are respectively arranged on both sides of the top of the n-type drift layer, a p+ type source region and an n+ type source region are wrapped in the p-type base region, the p+ type source region and the n+ type source region are arranged side by side and contact each other at the sides, and the p+ type source region is arranged close to the side of the n-type drift layer; a first source metal layer, an oxide layer and a second source metal layer are arranged in sequence from left to right above the n-type drift layer, a polysilicon gate is wrapped in the oxide layer, a gate oxide layer adjacent to the polysilicon gate is arranged below the oxide layer, and the cross section of the polysilicon gate is H-shaped; a top metal layer is arranged above the first source metal layer, the oxide layer and the second source metal layer, and a passivation layer is arranged above the top metal layer.

2. The silicon carbide based H-gate power device according to claim 1, characterized in that: The depth of the p-type base region is 1.5 μm and the doping concentration is 1e17 cm -3 ~1e18 cm -3 The depth of the n+ type source region is 0.2 μm, and the doping concentration is greater than 1e19 cm -3 The depth of the p+ source region is 3.0 μm and the doping concentration is 1e18 cm -3 ~1e19 cm -3 .

3. The silicon carbide based H-gate power device according to claim 1, characterized in that: The thickness of the gate oxide layer is 500 Å.

4. The silicon carbide based H-gate power device according to claim 1, characterized in that: The thickness of the polysilicon gate is 4000A.

5. The silicon carbide based H-gate power device according to claim 1, characterized in that: The thickness of the oxide layer is 1.0 μm.

6. The silicon carbide based H-gate power device according to claim 1, characterized in that: The passivation layer includes a plasma enhanced tetraethyl orthosilicate layer with a thickness of 6000 Å, a plasma enhanced silicon nitride layer with a thickness of 300 Å, and a polyimide film layer with a thickness of 7 μm.

7. The silicon carbide based H-gate power device according to claim 1, characterized in that: The thickness of the first source metal layer and the second source metal layer are both 1000 Å.

8. The silicon carbide based H-gate power device according to claim 1, characterized in that: The thickness of the top metal layer is 4 μm.

9. The silicon carbide based H-gate power device according to claim 1, characterized in that: The back drain metal layer includes a metal titanium layer with a thickness of 1000A, a metal nickel layer with a thickness of 2000A, and a metal silver layer with a thickness of 10kA.

10. A method for preparing a silicon carbide-based H-gate power device according to any one of claims 1 to 9, comprising: Step S1: epitaxially growing an n-type drift layer on an n+ silicon carbide substrate; Step S2: forming a p-type base region on the n-type drift layer by sequentially growing a first masking layer process, a high temperature oxidation process, a photolithography process, an etching process, and an ion implantation process; Step S3: using the first masking layer to grow a layer of low-pressure tetraethoxy silicate glass, and forming an n+ type source region through a plasma dry isotropic etching process, a self-alignment process and an ion implantation process; Step S4: removing the first masking layer by wet method, re-depositing the second masking layers of each layer, and forming a p+ type source region by photolithography, etching and ion implantation; Step S5: growing a gate oxide layer through a carbon film growth and high temperature activation process and a nitrogen annealing process; Step S6: depositing saturated doped polysilicon on the gate oxide layer, and forming a polysilicon gate through photolithography and etching processes, wherein the cross section of the polysilicon gate is H-shaped; Step S7: depositing a layer of borophosphosilicate glass on the polysilicon gate and the gate oxide layer, and forming an oxide layer through photolithography and etching processes; Step S8: forming a first source metal layer and a second source metal layer on both sides of the oxide layer by a metal deposition process and a rapid annealing process; Step S9: forming a top metal layer through a sputtering process and an etching process, and depositing a passivation layer on the top metal layer; Step S10: forming a back drain metal layer on the back of the n+ type silicon carbide substrate by a metal deposition process and a laser annealing process, thereby completing the preparation of a silicon carbide-based H-type gate power device.