Solar cell preparation method and solar cell

The silicon matrix is ​​subjected to phosphorus ion implantation and coating printing and sintering through prefabricated tooling, which solves the problems of numerous processes and tail fluid treatment in the prior art, and improves the production efficiency and quality of solar cells.

CN118943235APending Publication Date: 2024-11-12DAS SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310536767.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing preparation process of selective emitter solar cells, there are many process processes and strict process control requirements. Cleaning and etching produces a large amount of acid and alkali tail fluid, which increases production costs.

Method used

Prefabricated tooling is used to implant phosphorus ions on the silicon matrix to form different doping layers, simplify the process operation process, avoid the production of tail fluid, and obtain solar cells through coating and printing sintering.

Benefits of technology

Effectively simplify process operations, reduce production costs, improve the quality and production efficiency of solar cells, and facilitate process control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943235A_ABST
    Figure CN118943235A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a solar cell and the solar cell. The preparation method of the solar cell comprises the following steps: texturing a silicon substrate to obtain a silicon substrate; the silicon substrate is subjected to phosphorus ion implantation through a prefabrication tool, so that a first doping layer is formed in a first doping area on the surface of the silicon substrate, a second doping layer is formed in a second doping area on the surface of the silicon substrate, and the phosphorus atom concentration of the first doping layer is larger than that of the second doping layer; and coating, printing and sintering the silicon substrate to obtain the solar cell, the preset tool comprises a tool body, a plurality of first injection holes and a plurality of second injection holes are formed in the tool body in the first direction, the first injection holes and the second injection holes are alternately formed in the second direction, and the second direction is perpendicular to the first direction; in the first direction, the length of the first injection hole is larger than that of the second injection hole; the first material injection hole is used for injecting phosphorus ions into the first doped region, and the second material injection hole is used for injecting phosphorus ions into the second doped region.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of photovoltaic technology, and specifically relates to a method for preparing a solar cell and a solar cell. Background Art

[0002] Solar cell technology is the most promising and practical new energy industry in the world. It is highly valued by governments of various countries and is the focus of new energy research and development of scientific research institutions in various countries. For conventional production solar cells, if you want to obtain a higher short-circuit current density, you need to obtain a light doping concentration and a shallow node depth; and to obtain a higher open-circuit voltage, you need a higher surface doping concentration. At the same time, a higher doping concentration is conducive to obtaining a better ohmic contact and reducing the series resistance of the battery. The selective emitter solar cell structure can better balance the above requirements, but the previous selective emitter solar cells have problems with low photogenerated carrier collection efficiency and light absorption efficiency, and often even have a "dead layer" phenomenon due to excessive surface concentration.

[0003] In the related art, the preparation process of selective emitter solar cells mainly adopts the laser doping process, which forms a phosphorus layer by diffusion on the surface of the silicon wafer, and then uses the laser for local doping, and then uses the solution to clean and etch the silicon wafer to form a doping layer with different doping concentrations on the surface of the silicon wafer. However, the use of this laser doping process requires more process flows, strict process control requirements, and cleaning and etching will produce a large amount of acid and alkali tail liquid, and the treatment of the tail liquid increases the production cost. Summary of the invention

[0004] The present application aims to provide a method for preparing a solar cell and a solar cell, at least to solve the problem in the related art that a laser doping process is used to prepare a selective emitter solar cell, which has many process steps and strict requirements on process control, and a large amount of acid and alkali tail liquid will be generated during cleaning and etching, and the treatment of the tail liquid increases the production cost.

[0005] In order to solve the above technical problems, this application is implemented as follows:

[0006] In a first aspect, an embodiment of the present application provides a method for preparing a solar cell, comprising:

[0007] Texturing the silicon substrate to obtain a silicon matrix;

[0008] Using a prefabricated tool to implant phosphorus ions into the silicon substrate, so as to form a first doping layer in a first doping region on the surface of the silicon substrate, and to form a second doping layer in a second doping region on the surface of the silicon substrate, wherein the phosphorus atom concentration of the first doping layer is greater than that of the second doping layer;

[0009] The silicon substrate is subjected to coating, printing and sintering to obtain a solar cell;

[0010] Among them, the preset tooling includes a tooling body, and a plurality of first injection holes and second injection holes extending along a first direction are opened on the tooling body, and the first injection holes and the second injection holes are alternately arranged along a second direction, and the second direction is perpendicular to the first direction; along the first direction, the length of the first injection hole is greater than the length of the second injection hole; the first injection hole is used to inject phosphorus ions into the first doping region, and the second injection hole is used to inject phosphorus ions into the second doping region.

[0011] Optionally, the step of implanting phosphorus ions into the silicon substrate using a prefabricated tool to form a first doping layer in a first doping region on the surface of the silicon substrate, and forming a second doping layer in a second doping region on the surface of the silicon substrate, comprises:

[0012] Installing the prefabricated tooling in a chamber of an ion implantation device, and connecting a traction voltage to the prefabricated tooling;

[0013] Under a first preset condition, the silicon substrate is passed from below the prefabricated tooling along the first direction to respectively inject phosphorus ions into the first doping region and the second doping region;

[0014] Under a second preset condition, the silicon substrate is annealed to form the first phosphorus-doped layer in the first doping region and the second phosphorus-doped layer in the second doping region.

[0015] Optionally, the first preset conditions include: phosphine flow rate is 10-15 sccm / min, radio frequency power is 800-1200W, and pulling voltage is 10KV; and / or,

[0016] The second preset conditions include: temperature of 820-880° C., pressure of 500-800 mbar, nitrogen flow rate of 5000-10000 sccm / min, and time of 30-50 min.

[0017] Optionally, the phosphorus atomic concentration of the first doping layer is 8 to 10E20 / cm 3 ; and / or, the phosphorus atomic concentration of the second doping layer is 2 to 4E20 / cm 3 .

[0018] Optionally, along the first direction, the length of the first injection hole is H cm, and the length of the second injection hole is h cm, satisfying: 2≤H / h≤4.

[0019] Optionally, a length H cm of the first injection hole satisfies: 12≤H≤15.

[0020] Optionally, the length h cm of the second injection hole satisfies: 3≤h≤5.

[0021] Optionally, along the second direction, the width of the first injection hole is D mm, satisfying: 0.1≤D≤0.2; and / or,

[0022] Along the second direction, the width of the second injection hole is d mm, satisfying: 1≤d≤2.

[0023] Optionally, the step of coating, printing and sintering the silicon substrate to obtain a solar cell comprises:

[0024] The front and back sides of the silicon substrate are respectively subjected to coating treatment to form silicon nitride layers on the front and back sides of the silicon substrate, wherein the thickness of the silicon nitride layer on the front side is 75 to 85 nm, and the thickness of the silicon nitride layer on the back side is 78 to 90 nm;

[0025] The slurry is printed at the corresponding position of the first doping layer by screen printing, and then sintered to obtain a solar cell.

[0026] In a second aspect, an embodiment of the present application provides a solar cell, which is manufactured using any of the solar cell manufacturing methods described above.

[0027] In an embodiment of the present application, a silicon substrate is textured to obtain a silicon substrate, and phosphorus ions are implanted into the silicon substrate using a prefabricated tool to form a first doping layer in a first doping area on the surface of the silicon substrate, and a second doping layer in a second doping area on the surface of the silicon substrate, wherein the phosphorus atom concentration of the first doping layer is greater than the phosphorus atom concentration of the second doping layer, and the silicon substrate is plated and printed and sintered to obtain a solar cell. Among them, a plurality of first injection holes and a plurality of second injection holes are opened along a first direction on the tool body of the preset tool, and the silicon substrate passes under the preset tool along the first direction, and phosphorus ions pass through the first injection hole and the second injection hole on the tool body to impact the surface of the silicon substrate, so as to inject phosphorus ions into the surface of the silicon substrate. Due to the different lengths of the first injection hole and the second injection hole, the phosphorus ion impact time received by different regions of the silicon substrate is different, thereby correspondingly forming doping layers with different phosphorus ion concentrations in different doping areas on the surface of the silicon substrate. The preparation method of the present application can effectively simplify the process operation flow and avoid the generation of tail liquid during the doping process, which can not only improve production efficiency but also save production costs, facilitate process control, and improve the quality of solar cells.

[0028] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0030] Figure 1 is a flow chart of a method for preparing a solar cell according to an embodiment of the present application;

[0031] Figure 2 is a schematic diagram of a prefabricated tooling according to an embodiment of the present application;

[0032] Figure 3 is a working principle diagram of a prefabricated tooling according to an embodiment of the present application;

[0033] Figure 4 is a flow chart of another method for preparing a solar cell according to an embodiment of the present application.

[0034] Reference numerals:

[0035] 100: tooling body; 101: electrode sheet; 110: first injection hole; 120: second injection hole; 200: silicon substrate; X: first direction; Y: second direction. DETAILED DESCRIPTION

[0036] The exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although the exemplary embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can also be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.

[0037] refer to Figure 1 , shows a flow chart of a method for preparing a solar cell provided in an embodiment of the present application. Figure 1 The method for preparing a solar cell shown comprises:

[0038] Step 101 , texturing a silicon substrate to obtain a silicon base 200 .

[0039] In the embodiment of the present application, a double-sided texturing operation is performed on the silicon substrate to form a velvet surface on the front and back sides of the silicon substrate, thereby obtaining a silicon substrate 200 having a velvet surface with a preset reflectivity. In the texturing operation procedure, velvet surfaces with different reflectivities can be obtained by adjusting the process parameters. The preset reflectivity can be set according to actual needs and is not limited here.

[0040] Step 102: Use a prefabricated tool to implant phosphorus ions into the silicon substrate 200 to form a first doping layer in a first doping region on the surface of the silicon substrate 200, and a second doping layer in a second doping region on the surface of the silicon substrate 200, wherein the phosphorus atom concentration of the first doping layer is greater than that of the second doping layer.

[0041] like Figure 2 and Figure 3 As shown, the preset tooling includes a tooling body 100, on which a plurality of first injection holes 110 and second injection holes 120 extending along a first direction X are provided, and the first injection holes 110 and the second injection holes 120 are alternately arranged along a second direction Y, and the second direction Y is perpendicular to the first direction X; along the first direction X, the length of the first injection holes 110 is greater than the length of the second injection holes 120; the first injection holes 110 are used to inject phosphorus ions into the first doping region, and the second injection holes 120 are used to inject phosphorus ions into the second doping region. Wherein, along the second direction Y, the first injection holes 110 and the second injection holes 120 are connected to each other.

[0042] In an embodiment of the present application, before performing the phosphorus ion implantation operation, a preset tooling is first installed in the chamber of the ion implantation equipment. The preset tooling can separate the chamber into a first cavity and a second cavity. The first cavity is located above the preset tooling, and the second cavity is located below the preset tooling.

[0043] During the phosphorus ion implantation operation on the silicon substrate 200, a process gas is introduced into the first cavity, the process gas includes phosphine, and under the preset radio frequency power, the phosphine is ionized to produce negatively charged phosphorus ions, and at the same time, a voltage is connected to the preset tooling, and the phosphorus ions are accelerated to impact the preset tooling under the action of the forward voltage, and the phosphorus ions will pass through the first injection hole 110 and the second injection hole 120 to enter the second cavity. Then, the silicon substrate 200 in step 101 passes through the second cavity along the first direction X, and the phosphorus ions passing through the first injection hole 110 and the second injection hole 120 will form a doping layer on the surface of the silicon substrate 200.

[0044] It can be understood that the lengths of the first injection hole 110 and the second injection hole 120 on the preset tooling in the present application along the first direction X are different, so that the concentration of phosphorus atoms doped in different areas on the silicon substrate 200 can be controlled. Among them, along the moving direction of the silicon substrate 200, since the length of the first injection hole 110 is relatively long, when the silicon substrate 200 passes under the first injection hole 110, the phosphorus ion impact time received by the corresponding area on the surface of the silicon substrate 200 is long, and thus, the phosphorus atom doping concentration in the corresponding area is high. The length of the second injection hole 120 is relatively short, and the phosphorus ion impact time received by the corresponding area on the surface of the silicon substrate 200 is short, and the phosphorus atom doping concentration in the corresponding area is low.

[0045] In a specific application, the area on the silicon substrate 200 corresponding to the first injection hole 110 is the first doping area, and the area corresponding to the second injection hole 120 is the second doping area. The first doping area is the area corresponding to the arrangement of the gate line. By forming a first doping layer with a higher concentration of phosphorus atoms in the first doping area, and then printing the gate line on the first doping layer, the ohmic contact between the gate line and the silicon substrate 200 can be improved. The second doping area corresponds to the emitter junction area, and controlling the second doping area to form a second doping layer with a lower concentration of phosphorus atoms can reduce the surface recombination of the emitter junction area.

[0046] Alternatively, if Figure 2 As shown, the length of the first injection hole 110 set along the first direction X is H cm, and the length of the second injection hole 120 set along the first direction X is h cm, satisfying: 2≤H / h≤4. Specifically, H / h can be set to any ratio of 2, 2.3, 2.5, 2.7, 3, 3.4, 3.5, 3.8, 4, etc.

[0047] Preferably, the length H of the first injection hole 110 may be set to be 3 times the length h of the second injection hole 120 .

[0048] In the embodiment of the present application, by setting the length ratio of the first injection hole 110 and the second injection hole 120 along the first direction X, during the ion implantation operation, the length of time that the first doping region and the second doping region are impacted by phosphorus ions can be correspondingly controlled, thereby accurately controlling the phosphorus atom concentrations of the obtained first doping layer and the second doping layer.

[0049] Alternatively, if Figure 2 As shown, the length H cm of the first injection hole 110 satisfies: 12≤H≤15. Specifically, the length H of the first injection hole 110 can be set to: 12 cm, 13 cm, 14 cm, 15 cm, etc.

[0050] Alternatively, if Figure 2 As shown, the length h cm of the second injection hole 120 satisfies: 3≤h≤5. Specifically, the length h of the second injection hole 120 can be set to: 3 cm, 3.5 cm, 4 cm, 4.5 cm, 5 cm, etc.

[0051] Alternatively, if Figure 2 As shown, along the second direction Y, the width of the first injection hole 110 is D mm, satisfying: 0.1≤D≤0.2. Specifically, the width D of the first injection hole 110 can be set to: 0.1mm, 0.13mm, 0.15mm, 0.16mm, 0.18mm, 0.2mm, etc.

[0052] The width D of the first injection hole 110 can be determined according to the width of the gate line of the solar cell to be manufactured. The width D of the first injection hole 110 is greater than or equal to the width of the gate line, thereby ensuring that the gate line matches the first doping layer.

[0053] Alternatively, if Figure 2 As shown, along the second direction Y, the width of the second injection hole 120 is d mm, satisfying: 1≤d≤2. Specifically, the width d of the second injection hole 120 can be set to: 1mm, 1.2mm, 1.4mm, 1.5mm, 1.7mm, 1.9mm, 2mm, etc.

[0054] The width of the second injection hole 120 can be determined according to the distance between two adjacent grid lines of the solar cell, and the second doping layer on the surface of the silicon substrate 200 is located between the grid lines.

[0055] It should be noted that the number of the first injection holes 110 and the second injection holes 120 in the preset tooling can match the number of grid lines on the surface of the solar cell to be prepared, and the specific number can be set according to actual needs, which is not limited in the embodiment of the present application.

[0056] In some embodiments, Figure 3 As shown, the tooling body 100 of the preset tooling in the present application includes three layers of electrode sheets 101, and the three layers of electrode sheets 101 have the same structure. Each layer of electrode sheets 101 is provided with the first injection hole 110 and the second injection hole 120. The three layers of electrode sheets 101 are stacked along a third direction to form a preset tooling, and the third direction is perpendicular to the first direction X and the second direction Y, respectively.

[0057] During the ion implantation operation, the three layers of electrode sheets 101 are respectively connected to the inner wall of the chamber of the ion implantation equipment, and there is a certain gap between the three layers of electrode sheets 101. Among them, the top layer of electrode sheet 101 is connected to the positive electrode of the power supply, the middle layer of electrode sheet 101 is connected to the negative electrode of the power supply, and the bottom layer of electrode sheet 101 is grounded. In this way, an electric field is generated in the preset tooling, and under the action of the electric field, negatively charged phosphorus ions can be pulled to move toward the preset tooling at high speed, and then pass through the injection holes in the preset tooling to impact the surface of the silicon substrate 200, thereby forming phosphorus atom doping on the surface of the silicon substrate 200.

[0058] Optionally, each layer of electrode sheets 101 in the preset tooling is made of a conductive material, for example, a graphite material, so that the preset tooling has conductive properties. By connecting each layer of electrode sheets 101 in the preset tooling to a voltage, an electric field can be generated in the preset tooling to pull the ionized negatively charged phosphorus ions through the first injection hole 110 and the second injection hole 120.

[0059] Step 103: coating, printing and sintering the silicon substrate 200 to obtain a solar cell.

[0060] Specifically, after forming a passivation film by coating the surface of the silicon substrate 200, a paste is printed on a corresponding position of the first doping layer and sintered to form a gate line, thereby manufacturing a solar cell.

[0061] In the embodiment of the present application, a silicon substrate is textured to obtain a silicon substrate 200, and a prefabricated tool is used to implant phosphorus ions into the silicon substrate 200 to form a first doping layer in a first doping region on the surface of the silicon substrate 200, and a second doping layer in a second doping region on the surface of the silicon substrate 200, wherein the phosphorus atom concentration of the first doping layer is greater than the phosphorus atom concentration of the second doping layer, and the silicon substrate 200 is plated and printed and sintered to obtain a solar cell. Among them, a plurality of first injection holes 110 and a plurality of second injection holes 120 are opened along the first direction X on the tool body 100 of the preset tool, and the silicon substrate 200 passes under the preset tool along the first direction X, and the phosphorus ions pass through the first injection holes 110 and the second injection holes 120 on the tool body 100 and impact the surface of the silicon substrate 200, so as to implant phosphorus ions on the surface of the silicon substrate 200. Since the lengths of the first injection hole 110 and the second injection hole 120 are different, the phosphorus ion impact time received by different regions of the silicon substrate 200 is different, thereby corresponding to the formation of doping layers with different phosphorus ion concentrations in different doping regions on the surface of the silicon substrate 200. The preparation method of the present application can effectively simplify the process operation flow, and at the same time avoid the generation of tail liquid during the doping process, which can not only improve production efficiency, but also save production costs, and facilitate process control and improve the quality of solar cells.

[0062] refer to Figure 4 , Figure 4 Another method for preparing a solar cell provided in an embodiment of the present application is shown, which may specifically include the following steps:

[0063] Step 201: Place the silicon substrate in a strong alkaline solution to perform double-sided texturing to obtain a silicon substrate 200 with a texturing reflectivity of 9% to 10%.

[0064] Specifically, the strong alkaline solution includes: a potassium hydroxide solution with a concentration of 3-7% and a texturing additive with a concentration of 1-2%. The texturing additive includes: 15-30 wt.% isopropyl alcohol, 2-4 wt.% sodium hydroxide, and 50-70 wt.% water.

[0065] The silicon substrate is textured by placing the silicon substrate in a strong alkaline solution to form a velvet surface on the front and back of the silicon substrate, thereby obtaining a silicon substrate 200 with a velvet surface, wherein the reflectivity of the velvet surface is 9% to 10%. Optionally, the reflectivity of the velvet surface can be set to 9%, 9.2%, 9.5%, 9.7%, 10%, etc.

[0066] Step 202: Install the prefabricated tooling in a chamber of an ion implantation device, and connect a traction voltage to the prefabricated tooling.

[0067] Specifically, the prefabricated tooling is installed in the chamber of the ion implantation device, and the chamber is divided into a first cavity and a second cavity by the prefabricated tooling, wherein the first cavity is located above the prefabricated tooling and the second cavity is located below the prefabricated tooling. At the same time, the prefabricated tooling is connected to the traction voltage, and the upper electrode sheet 101 of the prefabricated tooling is connected to the positive electrode of the power supply, the middle electrode sheet 101 is connected to the negative electrode of the power supply, and the lower electrode sheet 101 is grounded, thereby generating an electric field in the prefabricated tooling.

[0068] Step 203 : Under a first preset condition, the silicon substrate 200 is passed below the prefabricated tooling along the first direction X to respectively implant phosphorus ions into the first doping region and the second doping region.

[0069] Specifically, phosphine is introduced into the first cavity of the ion implantation device, and the corresponding radio frequency power is set so that the phosphine is ionized to generate negatively charged phosphorus ions, and under the pulling electric field of the preset tooling, the phosphorus ions pass through the first injection hole 110 and the second injection hole 120. At the same time, the silicon substrate 200 is passed from the second cavity to the bottom of the preset tooling along the first direction X, so that the negatively charged phosphorus ions will impact different areas of the surface of the silicon substrate 200 accordingly, thereby respectively injecting phosphorus ions into the first doping area and the second doping area of ​​the silicon substrate 200.

[0070] Specifically, the first preset conditions include: phosphine flow rate is 10-15 sccm / min, radio frequency power is 800-1200W, and pulling voltage is 10KV.

[0071] Among them, the phosphine flow rate can be set to any value such as 10sccm / min, 11sccm / min, 12sccm / min, 13sccm / min, 14sccm / min, 15sccm / min, etc.

[0072] Among them, the RF power can be set to any value such as 800W, 900W, 1000W, 1100W, 1200W, etc.

[0073] Step 204 , annealing the silicon substrate 200 under a second preset condition to form the first phosphorus-doped layer in the first doping region and the second phosphorus-doped layer in the second doping region.

[0074] Specifically, after the phosphorus atoms are implanted into the surface of the silicon substrate 200 , the silicon substrate 200 is further annealed to form a stable doping layer on the surface of the silicon substrate 200 .

[0075] The second preset conditions include: temperature of 820-880° C., pressure of 500-800 mbar, nitrogen flow rate of 5000-10000 sccm / min, and time of 30-50 min.

[0076] Specifically, the annealing temperature can be set to: 820°C, 830°C, 840°C, 850°C, 860°C, 870°C, 880°C, etc.

[0077] The pressure can be set to: 500mbar, 600mbar, 700mbar, 800mbar, etc.

[0078] In some embodiments, the phosphorus atomic concentration of the first doping layer is 8 to 10E20 / cm3. Specifically, the phosphorus atomic concentration of the first doping layer can be set to: 8E20 / cm3, 8.5E20 / cm3, 9E20 / cm3, 9.5E20 / cm3, 10E20 / cm3, etc.

[0079] In some embodiments, the phosphorus atomic concentration of the second doping region is 2 to 4E20 / cm3. Specifically, the phosphorus atomic concentration of the second doping layer can be set to: 2E20 / cm3, 2.5E20 / cm3, 3E20 / cm3, 3.5E20 / cm3, 4E20 / cm3, etc.

[0080] Step 205, coating the front and back sides of the silicon substrate 200 to form silicon nitride layers on the front and back sides of the silicon substrate 200, respectively, wherein the thickness of the silicon nitride layer on the front side is 75-85 nm, and the thickness of the silicon nitride layer on the back side is 78-90 nm.

[0081] Specifically, a vapor deposition coating process may be used to form a silicon nitride passivation film with a corresponding thickness on the front and back sides of the silicon substrate 200 .

[0082] The thickness of the silicon nitride layer on the front side of the silicon substrate 200 can be set to 75 nm, 76 nm, 78 nm, 80 nm, 82 nm, 85 nm, etc.

[0083] The thickness of the silicon nitride layer on the back side of the silicon substrate 200 can be set to 78 nm, 80 nm, 83 nm, 85 nm, 88 nm, 90 nm, etc.

[0084] Step 206: Print paste at a position corresponding to the first doping layer by screen printing, and sinter the paste to obtain a solar cell.

[0085] Specifically, the paste is printed at a position corresponding to the first doping layer on the silicon substrate 200 by screen printing, and then the paste is sintered to form a grid line on the first doping layer, thereby preparing a solar cell.

[0086] The sintering temperature is 740-800°C, and the sintering time is 30-60s. Specifically, the sintering temperature can be set to 740°C, 750°C, 780°C, 800°C, etc. The sintering time can be set to 30s, 35s, 40s, 45s, 50s, 55s, 60s, etc.

[0087] It should be noted that the specific process steps of using screen printing slurry can be made by referring to the screen printing process in the relevant technology, and the embodiments of the present application will not be repeated here.

[0088] In the embodiment of the present application, a silicon substrate is textured to obtain a silicon substrate 200, and a prefabricated tool is used to implant phosphorus ions into the silicon substrate 200 to form a first doping layer in a first doping region on the surface of the silicon substrate 200, and a second doping layer in a second doping region on the surface of the silicon substrate 200, wherein the phosphorus atom concentration of the first doping layer is greater than the phosphorus atom concentration of the second doping layer, and the silicon substrate 200 is plated and printed and sintered to obtain a solar cell. Among them, a plurality of first injection holes 110 and a plurality of second injection holes 120 are opened along the first direction X on the tool body 100 of the preset tool, and the silicon substrate 200 passes under the preset tool along the first direction X, and the phosphorus ions pass through the first injection holes 110 and the second injection holes 120 on the tool body 100 and impact the surface of the silicon substrate 200, so as to implant phosphorus ions on the surface of the silicon substrate 200. By controlling the process conditions of ion implantation, a doping layer with a phosphorus atom concentration is formed on the surface of the silicon substrate 200, so that the phosphorus atom concentration of the first doping layer corresponding to the printed grid line on the silicon substrate surface is high, and the phosphorus atom concentration of the second doping layer corresponding to the emission junction area is low. In this way, the ohmic contact between the silicon substrate surface and the grid line can be ensured, and the surface metal recombination of the emission junction area can be reduced, thereby improving the open circuit voltage and fill factor of the solar cell. The preparation method of the present application can effectively simplify the process operation flow, and at the same time avoid the generation of tail liquid during the doping process, which can not only improve production efficiency, but also save production costs, and facilitate process control and improve the quality of solar cells.

[0089] Example 1

[0090] This embodiment provides a method for preparing a solar cell, which mainly includes the following steps:

[0091] S1. The silicon wafer is subjected to a texturing solution to obtain a silicon substrate with a texturing reflectivity of 9.5%. The texturing solution includes: a KOH solution with a concentration of 6.5% and a texturing additive with a concentration of 1.5%.

[0092] S2. Place the silicon substrate in S1 into an ion implantation device equipped with a preset tool. The raw material is phosphine at 12 sccm / min. Under an RF power of 1100W, phosphine is ionized into negatively charged phosphorus ions. Connect the preset tool to a voltage of 10KV to implant phosphorus on the silicon wafer surface.

[0093] S3: anneal the silicon substrate in S2 at a temperature of 855°C, a nitrogen flow rate of 5000sccm / min, a pressure of 800mbar, and a time of 35min, so that the phosphorus atomic concentration in the heavily doped area is 9.6E20 / cm 3 The phosphorus atomic concentration in the emitter junction is 3.6E20 / cm 3 .

[0094] S4. The silicon substrate in S3 is subjected to a front-side silicon nitride coating treatment, wherein the thickness of the silicon nitride is 78 nm.

[0095] S5. The silicon substrate in S4 is subjected to a back side silicon nitride coating treatment, wherein the thickness of the silicon nitride is 82 nm.

[0096] S6. Screen printing and sintering are performed on the silicon substrate in S5, with the sintering temperature being 785° C. and the sintering time being 40 seconds, to obtain a solar cell.

[0097] Comparative Example 1

[0098] S1. The silicon wafer is subjected to a texturing solution to obtain a silicon substrate with a texturing reflectivity of 9.5%. The texturing solution includes: a KOH solution with a concentration of 6.5% and a texturing additive with a concentration of 1.5%.

[0099] S2. Diffusion of phosphorus oxychloride into the silicon substrate in S1, with a deposition temperature of 780° C., a deposition time of 10 min, a pressure of 80 mbar, a flow rate of nitrogen carrying phosphorus oxychloride of 800 sccm / min, and an oxygen of 600 sccm / min.

[0100] S3, the silicon substrate in S2 is heated to 870°C and pushed forward for 20 minutes at a pressure of 200 mabr; the surface concentration is 4.3E20 / cm 3 .

[0101] S4. Performing back alkali polishing on the silicon substrate in S3, with 8% KOH solution, 3.5 L additives, 450 L water, temperature 73° C., and time 200 s.

[0102] S5. Annealing the silicon substrate in S4 at a temperature of 700° C., a time of 30 min, an oxygen flow rate of 3000 sccm / min, and a pressure of 800 mbar.

[0103] S6, coating the front side of the S5 silicon substrate with silicon nitride, the thickness of the silicon nitride being 78nm;

[0104] S7, performing silicon nitride coating on the back of the S6 silicon substrate, the thickness of the silicon nitride being 82nm;

[0105] S8. Screen printing and sintering are performed on the silicon substrate in S7, with the sintering temperature being 785° C. and the sintering time being 40 seconds, to obtain a solar cell.

[0106] The solar cells prepared in Example 1 and Comparative Example 1 were tested, and the results are shown in Table 1:

[0107] Table 1

[0108] Group quantity Eta(%) Uoc(V) Isc(A) FF(%) Example 1 2100 23.47 0.6943 13.882 81.33 Comparative Example 1 1700 23.32 0.6912 13.890 81.12

[0109] As can be seen from Table 1, the preparation method of the present application significantly reduces the number of steps compared to the preparation method of Comparative Example 1, which helps to improve production efficiency, eliminates the cleaning and etching steps, and reduces the generation of acid and alkali tail liquid. At the same time, the solar cell prepared by the preparation method of the present application can increase the open circuit voltage by 3.1mV and the fill factor by 0.21%.

[0110] It can be understood that the solar cell prepared by the preparation method of the embodiment of the present application can accurately control the concentration of phosphorus atoms in different doping areas, so that the surface of the solar cell is heavily doped with phosphorus atoms in the area in contact with the printed paste, thereby improving the ohmic contact of the corresponding area and increasing the metal composite of the silicon substrate and the paste from 450fA / cm 2 Reduced to 280fA / cm 2 , thereby improving the open circuit voltage and fill factor of solar cells.

[0111] In the above embodiments, it can be implemented in whole or in part by software, hardware, firmware or any combination thereof. When implemented by software, it can be implemented in whole or in part in the form of a computer program product. The computer program product includes one or more computer instructions. When the computer program instructions are loaded and executed on a computer, the process or function described in the embodiment of the present invention is generated in whole or in part. The computer can be a general-purpose computer, a special-purpose computer, a computer network, or other programmable device. The computer instructions can be stored in a computer-readable storage medium, or transmitted from one computer-readable storage medium to another computer-readable storage medium. For example, the computer instructions can be transmitted from a website site, computer, server or data center to another website site, computer, server or data center by wired (e.g., coaxial cable, optical fiber, digital subscriber line (DSL)) or wireless (e.g., infrared, wireless, microwave, etc.). The computer-readable storage medium can be any available medium that a computer can access or a data storage device such as a server or data center that includes one or more available media integrated. The available medium can be a magnetic medium (e.g., a floppy disk, a hard disk, a tape), an optical medium (e.g., a DVD), or a semiconductor medium (e.g., a solid-state hard disk Solid State Disk (SSD)), etc.

[0112] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0113] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. For the embodiments of the device, electronic device, computer-readable storage medium and computer program products containing instructions, since they are basically similar to the method embodiments, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiments.

[0114] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.

Claims

1. A method for preparing a solar cell, characterized in that: include: Texturing the silicon substrate to obtain a silicon matrix; Using a prefabricated tool to implant phosphorus ions into the silicon substrate, so as to form a first doping layer in a first doping region on the surface of the silicon substrate, and to form a second doping layer in a second doping region on the surface of the silicon substrate, wherein the phosphorus atom concentration of the first doping layer is greater than that of the second doping layer; The silicon substrate is subjected to coating, printing and sintering to obtain a solar cell; Wherein, the preset tooling comprises a tooling body, on which a plurality of first injection holes and second injection holes extending along a first direction are provided, the first injection holes and the second injection holes are alternately arranged along a second direction, and the second direction is perpendicular to the first direction; Along the first direction, the length of the first injection hole is greater than that of the second injection hole; the first injection hole is used to inject phosphorus ions into the first doping region, and the second injection hole is used to inject phosphorus ions into the second doping region.

2. The method for preparing a solar cell according to claim 1, characterized in that: The method of implanting phosphorus ions into the silicon substrate using a prefabricated tool to form a first doping layer in a first doping region on the surface of the silicon substrate and a second doping layer in a second doping region on the surface of the silicon substrate comprises: Installing the prefabricated tooling in a chamber of an ion implantation device, and connecting a traction voltage to the prefabricated tooling; Under a first preset condition, the silicon substrate is passed from below the prefabricated tooling along the first direction to respectively inject phosphorus ions into the first doping region and the second doping region; Under a second preset condition, the silicon substrate is annealed to form the first phosphorus-doped layer in the first doping region and the second phosphorus-doped layer in the second doping region.

3. The method for preparing a solar cell according to claim 2, characterized in that: The first preset conditions include: phosphine flow rate is 10-15 sccm / min, RF power is 800-1200W, and pulling voltage is 10KV; and / or, The second preset conditions include: temperature of 820-880° C., pressure of 500-800 mbar, nitrogen flow rate of 5000-10000 sccm / min, and time of 30-50 min.

4. The method for preparing a solar cell according to claim 1, characterized in that: The phosphorus atomic concentration of the first doping layer is 8 to 10E20 / cm 3 ; and / or, the phosphorus atomic concentration of the second doping layer is 2 to 4E20 / cm 3 .

5. The method for preparing a solar cell according to any one of claims 1 to 4, characterized in that: Along the first direction, the length of the first injection hole is H cm, and the length of the second injection hole is h cm, satisfying: 2≤H / h≤4.

6. The method for preparing a solar cell according to claim 5, characterized in that: The length Hcm of the first injection hole satisfies: 12≤H≤15.

7. The method for preparing a solar cell according to claim 5, characterized in that: The length hcm of the second injection hole satisfies: 3≤h≤5.

8. The method for preparing a solar cell according to claim 1, characterized in that: Along the second direction, the width of the first injection hole is D mm, satisfying: 0.1≤D≤0.2; and / or, Along the second direction, the width of the second injection hole is d mm, satisfying: 1≤d≤2.

9. The method for preparing a solar cell according to claim 1, characterized in that: The silicon substrate is subjected to coating, printing and sintering to obtain a solar cell, comprising: The front and back sides of the silicon substrate are respectively subjected to coating treatment to form silicon nitride layers on the front and back sides of the silicon substrate, wherein the thickness of the silicon nitride layer on the front side is 75 to 85 nm, and the thickness of the silicon nitride layer on the back side is 78 to 90 nm; The slurry is printed at the corresponding position of the first doping layer by screen printing, and then sintered to obtain a solar cell.

10. A solar cell, characterized in that: The solar cell is prepared by the method for preparing the solar cell according to any one of claims 1 to 9.