Photovoltaic cell metallization method, photovoltaic cell and preparation method thereof, and photovoltaic module

By printing phosphorus-silicon paste as a transition structure in Topcon cells, combined with pre-sintering and sintering processes, the problem of polycrystalline silicon layer burn-through was solved, improving field passivation effect and photoelectric conversion efficiency, while reducing cost.

CN118943246APending Publication Date: 2024-11-12JOLYWOOD (TAIZHOU) SOLAR TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411033460.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The thin polycrystalline silicon layer in existing Topcon cells is prone to localized burn-through of the polycrystalline silicon layer and tunnel oxide layer during aluminum or nickel paste sintering, which affects the field passivation effect, increases leakage current, and the use of silver paste is expensive, making it difficult to overcome the burn-through problem and affecting photoelectric conversion efficiency.

Method used

Phosphorus silicon paste is printed in the laser-grooved area as a transition structure, so that the N+ polycrystalline silicon layer comes into contact with the phosphorus silicon paste. After printing aluminum or nickel paste, a pre-sintering and sintering process is combined to form a symbiotic layer of phosphorus silicon and N+ polycrystalline silicon and an N++ microcrystalline silicon layer, which improves the field passivation effect and prevents burn-through.

Benefits of technology

It effectively prevents aluminum or nickel paste from burning through the polycrystalline silicon layer, ensures passivation effect, reduces battery leakage current, reduces parasitic light absorption, improves photoelectric conversion efficiency, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943246A_ABST
    Figure CN118943246A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of new energy, and discloses a photovoltaic cell metallization method, a photovoltaic cell, a preparation method of the photovoltaic cell and a photovoltaic module. The metallization method comprises the steps that laser selective etching is carried out, so that the antireflection film locally forms a laser slotting opening of a locally exposed N + polycrystalline silicon layer; printing silicon-phosphorus slurry in the laser grooving area, and drying the silicon-phosphorus slurry; locally printing aluminum paste (or nickel paste) on the surface of the dried silicon phosphorus slurry, and drying; and pre-sintering, sintering and cooling to enable the sintered first metal slurry to form a first electrode, and enabling the sintered silicon phosphorus slurry to sequentially form a co-melting layer of phosphorus silicon and N + polycrystalline silicon, an N + + microcrystalline silicon layer and an aluminum-silicon alloy (or nickel-silicon alloy) between the N + polycrystalline silicon layer and the first electrode. The metallization method can prevent the aluminum paste or the nickel paste from burning through, realize local phosphorus heavy doping, improve the passivation effect, help to thin the N + polycrystalline silicon layer, realize better conduction of electrons, reduce the cost and improve the battery efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new energy technology, and in particular to a photovoltaic cell metallization method, a photovoltaic cell and a preparation method thereof, and a photovoltaic module. Background Art

[0002] At present, Topcon cells have become the mainstream of photovoltaic cells. And further improving the photoelectric conversion efficiency of Topcon cells has also become the current main task. For existing Topcon cells (as shown in publication number CN117352589B), the N+ polysilicon layer (i.e., phosphorus-doped polysilicon layer) on the back of the tunneling oxide layer (i.e., tunneling silicon oxide layer) is partially heavily doped with an in-situ phosphorus source to form an N++ polysilicon layer (i.e., n++ highly heavily doped area), which can form a field passivation on the back of the silicon substrate while also forming a gettering effect, which helps the metallization area of ​​the subsequent battery to form a good contact, helps to reduce the contact resistance, and then helps to improve the photoelectric conversion efficiency of the battery. However, a thicker polysilicon layer (as shown in publication number CN117352589B, the thickness of its intrinsic amorphous silicon layer is 80-200nm, and correspondingly, the thickness of its polysilicon layer is also 80-200nm) is prone to parasitic light absorption, which is not conducive to improving the photoelectric conversion efficiency of the battery.

[0003] In practice, the thickness of the polysilicon layer on the back of the tunnel oxide layer is usually controlled at 90-110nm. When the thickness of the polysilicon layer (such as N+ polysilicon layer, N++ polysilicon layer) is further reduced, the thinner polysilicon layer can effectively reduce parasitic light absorption and reduce production costs. However, the thinner polysilicon layer can easily cause the aluminum paste or nickel paste to partially burn through the polysilicon layer (such as N+ polysilicon layer, N++ polysilicon layer) and the tunnel oxide layer during sintering, resulting in direct contact between the aluminum paste (or nickel paste) and the silicon substrate, thereby affecting the field passivation effect, resulting in a large battery leakage current, and increasing metal composites, all of which will reduce the battery's photoelectric conversion efficiency. And because the burn-through performance of aluminum paste (or nickel paste) is much greater than that of silver paste. Therefore, existing Topcon batteries usually use silver paste on the back to prepare the back electrode to improve the burn-through problem. However, silver paste is more expensive than aluminum paste (or nickel paste), which will greatly increase the cost of the back electrode; moreover, the thinner polysilicon layer combined with silver paste is difficult to effectively overcome the burn-through problem, and will still affect the field passivation effect on the back side, resulting in a larger battery leakage current and increased metal recombination, which is not conducive to further improving the battery's photoelectric conversion efficiency. Summary of the invention

[0004] The purpose of the present invention is to overcome the deficiencies of the prior art and to provide a photovoltaic cell metallization method, a photovoltaic cell and a preparation method thereof, and a photovoltaic module.

[0005] Based on this, the present invention discloses a photovoltaic cell metallization method, comprising the following steps:

[0006] S1. Prepare a silicon substrate, wherein a tunneling oxide layer, an N+ polysilicon layer and an anti-reflection film are sequentially provided on the surface of the silicon substrate;

[0007] S2, performing laser selective etching on the anti-reflection film to form laser notches in the local area of ​​the anti-reflection film that partially expose the N+ polysilicon layer;

[0008] S3, printing silicon-phosphorus slurry on the surface of the exposed N+ polysilicon layer, and drying, so that the dried silicon-phosphorus slurry covers the laser-cut notches;

[0009] S4, locally printing a first metal paste on the surface of the dried silicon-phosphorus paste, and drying it; the first metal paste is aluminum paste or nickel paste;

[0010] S5. The entire silicon substrate is pre-sintered and sintered in sequence, and cooled, so that the sintered first metal slurry forms a first electrode, and the sintered silicon-phosphorus slurry forms a eutectic layer of phosphorus silicon and N+ polycrystalline silicon, an N++ microcrystalline silicon layer and a first metal silicon alloy between the N+ polycrystalline silicon layer and the first electrode in sequence; the first metal silicon alloy is an aluminum silicon alloy or a nickel silicon alloy, and the first metal silicon alloy contacts the first electrode.

[0011] Preferably, in step S3, the silicon-phosphorus slurry is a mixture of silicon element, glass powder, phosphorus element, and an organic additive in a mass ratio of 11-16:2-7:1:1; the organic additive is an organic dispersant or a thixotropic agent;

[0012] The thickness of the dried silicon-phosphorus slurry is greater than the thickness of the anti-reflection film, and the width of the dried silicon-phosphorus slurry is greater than the width of the laser notch; the drying temperature of the silicon-phosphorus slurry is 200-400°C.

[0013] Further preferably, the thickness of the dried silicon-phosphorus slurry is at least 1 μm greater than the thickness of the anti-reflection film; and the width of the dried silicon-phosphorus slurry is at least 80 μm greater than the width of the laser-grooved opening.

[0014] Preferably, in step S4, the width of the first metal slurry after drying is smaller than the width of the silicon-phosphorus slurry after drying;

[0015] The drying temperature of the first metal slurry is 200-400°C.

[0016] Further preferably, the width of the first metal paste after drying is at least 20 μm smaller than the width of the silicon-phosphorus paste after drying.

[0017] Preferably, in step S5, the pre-sintering temperature is 300-550° C., and the pre-sintering time is 8-12 s; the sintering temperature is 600-700° C., and the sintering time is less than 1 s.

[0018] Further preferably, in step S1, the thickness of the N+ polysilicon layer is 50-100 nm (preferably 50-60 nm);

[0019] In step S3, before printing the silicon-phosphorus paste, it also includes: locally printing a second metal paste on the surface of the anti-reflection film and drying it; the first metal paste is a fine grid metal paste, and the second metal paste is a main grid metal paste.

[0020] The present invention also discloses a method for preparing a photovoltaic cell, comprising the following preparation steps:

[0021] Step 1: Prepare a P+ emitter on the front side of the silicon substrate;

[0022] Step 2: sequentially preparing a tunnel oxide layer and an N+ polysilicon layer on the back side of the silicon substrate;

[0023] Step 3: prepare a passivation anti-reflection film on the front side of the P+ emitter, and prepare an anti-reflection film on the back side of the N+ polysilicon layer;

[0024] Step 4: metallizing the silicon substrate processed in step 3 using the photovoltaic cell metallization method described above in the present invention; in step S5, before pre-sintering, it also includes: printing a front metal paste locally on the front side of the silicon substrate.

[0025] The present invention also discloses a photovoltaic cell, which is prepared by the photovoltaic cell preparation method described above in the present invention.

[0026] The present invention also discloses a photovoltaic assembly, which comprises the photovoltaic cell described above in the present invention.

[0027] Compared with the prior art, the present invention has at least the following beneficial effects:

[0028] The metallization method of the present invention prints phosphorus silicon paste as a transition structure in the laser grooved area before printing the first metal paste (aluminum paste or nickel paste), so that the N+ polysilicon layer can contact the phosphorus silicon paste, and after printing the aluminum paste (or nickel paste), the aluminum paste (or nickel paste) can also contact the phosphorus silicon paste, and then combine the pre-sintering and sintering processes. In this way, (1) during sintering, the phosphorus silicon paste can greatly improve the safety of aluminum paste (or nickel paste) sintering, effectively prevent the passivation structure from being destroyed due to the aluminum paste (or nickel paste) burning through the N+ polysilicon layer, etc., ensure the passivation effect, avoid battery leakage current, and reduce metal recombination.

[0029] (2) At the same time, the middle section of the sintered phosphorus silicon slurry can also achieve heavy phosphorus doping on the surface of the N+ polycrystalline silicon layer locally to form an N++ microcrystalline silicon layer, thereby improving the field passivation effect.

[0030] (3) Due to the burn-through barrier effect of phosphorus silicon paste on aluminum paste (or nickel paste), while improving the passivation effect, the N+ polysilicon layer can be further thinned (the N+ polysilicon layer can be thinned to 50-60nm), thereby reducing parasitic light absorption, increasing light utilization, and further increasing short-circuit current and improving the photoelectric conversion efficiency of the battery.

[0031] (4) After sintering, the phosphorus silicon slurry can sequentially form a eutectic layer of phosphorus silicon and N+ polysilicon (which contacts the N+ polysilicon layer), an N++ microcrystalline silicon layer and a first metal silicon alloy (which contacts the first electrode), so that electrons can be better conducted in the laser grooved area, thereby improving the electron transmission performance between the first electrode (such as an aluminum electrode or a nickel electrode) and the N+ polysilicon layer, and effectively reducing the contact resistivity.

[0032] (5) In addition, the metallization method of the present invention can also increase the printing width of aluminum paste (or nickel paste). The printing of large line width aluminum paste (or nickel paste) can reduce line resistance loss, significantly improve the FF (fill factor) of the battery, and improve the efficiency of the battery cell. In addition, aluminum paste (or nickel paste) is cheaper than silver paste, so it can also reduce costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic diagram of the cross-sectional structure of a silicon substrate after step 1 of a method for preparing a photovoltaic cell in this embodiment.

[0034] Figure 2 It is a schematic diagram of the cross-sectional structure of a silicon substrate after step 2 of the method for preparing a photovoltaic cell of this embodiment.

[0035] Figure 3 It is a schematic diagram of the cross-sectional structure of a silicon substrate after step 4 of the method for preparing a photovoltaic cell of this embodiment.

[0036] Figure 4 It is a schematic diagram of the cross-sectional structure of a silicon substrate after step 5 of the method for preparing a photovoltaic cell of this embodiment.

[0037] Figure 5 This is a schematic diagram of the cross-sectional structure of a silicon substrate after step 6 of the method for preparing a photovoltaic cell of this embodiment.

[0038] Figure 6 It is a schematic diagram of the cross-sectional structure of a silicon substrate after step 71 of the method for preparing a photovoltaic cell of this embodiment.

[0039] Figure 7It is a schematic diagram of the cross-sectional structure of a silicon substrate after step 72 of the method for preparing a photovoltaic cell of this embodiment.

[0040] Figure 8 It is a schematic diagram of the cross-sectional structure of a silicon substrate after step 73 of the method for preparing a photovoltaic cell of this embodiment.

[0041] Fig. 9 It is a schematic diagram of the cross-sectional structure of a silicon substrate after step 74 of the method for preparing a photovoltaic cell of this embodiment.

[0042] Explanation of the accompanying drawings: silicon substrate 1; P+ emitter 2; tunneling oxide layer 3; N+ polysilicon layer 4; Al2O3 film 5; front SiNx film 6; back SiNx film 7; laser notch 8; dried silicon-phosphorus slurry 9; eutectic layer of phosphorus silicon and N+ polysilicon 91; N++ microcrystalline silicon layer 92; fine gate metal silicon alloy 93; dried fine gate metal slurry 10; back electrode 11; front electrode 12. DETAILED DESCRIPTION

[0043] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0044] Example

[0045] A method for preparing a photovoltaic cell in this embodiment, see Figure 1-9 , comprising the following preparation steps:

[0046] Step 1: Perform double-sided texturing on the silicon substrate 1, so that both the front and back surfaces of the silicon substrate 1 form a pyramid-shaped texturing structure. The structure of the silicon substrate 1 after step 1 is as follows: Figure 1 shown.

[0047] In step 1, it is preferred to use an alkaline solution for double-sided texturing treatment; the alkaline solution includes but is not limited to a NaOH solution or a KOH solution.

[0048] Step 2: Perform a single-sided boron diffusion doping treatment on the silicon substrate 1 after the treatment in step 1 to form a P+ emitter 2 on the front side of the silicon substrate 1. The structure of the silicon substrate 1 after the treatment in step 2 is as follows: Figure 2 shown.

[0049] In step 2, a diffusion furnace is used to perform a single-sided boron diffusion doping treatment, and the doping source includes but is not limited to BBr3 or BCl3. The specific processing process of the single-sided boron diffusion doping treatment refers to the prior art, so it is not described in detail.

[0050] It should be noted that during the single-sided boron diffusion doping process in step 2, not only borosilicate glass (BSG) will be formed on the front side of the P+ emitter 2 of the silicon substrate 1, but also BSG may be formed on the left and right edges of the silicon substrate 1 and on the back side of the silicon substrate 1.

[0051] Step 3: performing etching and cleaning treatment on the silicon substrate 1 processed in step 2 to remove the BSG on the edge, front side and back side of the silicon substrate 1 .

[0052] In one example of this embodiment, in step 3, a mixed solution of HF and HNO3 is preferably used for etching and cleaning. Of course, in other examples of this embodiment, other acid solutions may also be used for etching and cleaning in step 3.

[0053] Step 4: Polish the back of the silicon substrate 1 after the treatment in step 3 to form a flat surface on the back of the silicon substrate 1. The structure of the silicon substrate 1 after the treatment in step 4 is as follows: Figure 3 shown.

[0054] In step 4, the polishing treatment is preferably an alkali polishing treatment.

[0055] In one example of this embodiment, in step 4, preferably TMAH solution (tetramethylammonium hydroxide solution) is used for alkali polishing. Of course, in other examples of this embodiment, other alkali solutions can also be used for alkali polishing in step 4.

[0056] Step 5: A tunneling oxide layer 3 and a phosphorus-doped polysilicon layer (the phosphorus-doped polysilicon layer is also referred to as an N+ polysilicon layer 4) are sequentially prepared on the back of the silicon substrate 1 processed in step 4. The structure of the silicon substrate 1 processed in step 5 is as follows: Figure 4 shown.

[0057] In step 5, the tunnel oxide layer 3 is preferably SiO2 with a thickness of 1-2 nm (eg, 1.5 nm).

[0058] In one example of this embodiment, in step 5, preferably, a PVD method (physical vapor deposition method) or a PECVD method (plasma enhanced chemical vapor deposition method) method is used to prepare the tunnel oxide layer 3. Of course, in other examples of this embodiment, step 5 can also use other existing deposition methods to prepare the tunnel oxide layer 3.

[0059] In step 5, the thickness of the N+ polysilicon layer 4 is 50-100 nm (preferably 50-60 nm).

[0060] In one example of this embodiment, in step 5, the N+ polysilicon layer 4 is preferably prepared by PVD method. Of course, in other examples of this embodiment, step 5 may also adopt other existing deposition methods to prepare the N+ polysilicon layer 4.

[0061] Step 6: prepare a passivation anti-reflection film and an anti-reflection film on the front and back sides of the silicon substrate 1 processed in step 5, respectively.

[0062] In step 6, the passivation anti-reflection film preferably includes an Al2O3 film 5 disposed on the front of the P+ emitter 2 and a front SiNx film 6 (front silicon nitride film) disposed on the front of the Al2O3 film 5; and the anti-reflection film is preferably a back SiNx film 7. The structure of the silicon substrate 1 after step 6 is as follows: Figure 5 shown.

[0063] In step 6, preferably, the Al2O3 film 5 is prepared by ALD (atomic layer deposition); preferably, the front SiNx film 6 and the back SiNx film 7 are prepared by PECVD (or other existing deposition methods).

[0064] Step 7: Using a photovoltaic cell metallization method as shown in the present embodiment, the silicon substrate 1 treated in step 6 is metallized to obtain the photovoltaic cell of the present embodiment (the photovoltaic cell structure is as shown in the following figure). Fig. 9 shown).

[0065] A photovoltaic cell metallization method according to this embodiment includes the following steps:

[0066] Step 71, laser selectively etch the anti-reflection film to remove the anti-reflection film corresponding to the fine gate metallization area (i.e., the back SiNx film 7), so that the local area of ​​the anti-reflection film (the local area of ​​the anti-reflection film corresponds to the fine gate metallization area) forms a laser notch 8 that can partially expose the N+ polysilicon layer 4. The structure of the silicon substrate 1 after step 71 is as follows: Figure 6 shown.

[0067] Step 72, print the main grid metal paste on the back of the anti-reflection film and dry it; then, print the silicon phosphorus paste on the laser slotted area and dry it, so that the thickness of the dried silicon phosphorus paste 9 is greater than the thickness of the anti-reflection film, and the width of the dried silicon phosphorus paste 9 is greater than the width of the laser slotted opening 8 (the dried silicon phosphorus paste 9 completely covers the laser slotted opening 8). The structure of the silicon substrate 1 after step 72 is as follows Figure 7 shown.

[0068] It should be noted that the laser grooved area in this embodiment includes the laser grooved opening 8 partially exposing the N+ polysilicon layer 4 , and the area outside the laser grooved opening 8 and the vicinity thereof.

[0069] In step 72, the main grid metal paste is preferably silver paste. The main grid metal paste and its printing process are all referred to the prior art, so they are not described in detail here.

[0070] In step 72, the silicon-phosphorus slurry is a mixture of silicon, glass powder, phosphorus, and an organic additive in a mass ratio of 11-16:2-7:1:1. The organic additive is an organic dispersant or a thixotropic agent. In the silicon-phosphorus slurry, silicon is a silicon single substance particle, and phosphorus is a phosphorus single substance particle. Silicon is mainly used to achieve contact with the N+ polysilicon layer 4 and the subsequently printed aluminum paste during subsequent sintering; phosphorus is mainly used to achieve selective heavy doping during subsequent sintering, so that the N++ microcrystalline silicon layer 92 (such as Fig. 9 As shown); glass powder is mainly used to reduce the melting temperature of silicon, thereby promoting the contact between silicon and the N+ polysilicon layer 4 during subsequent sintering; organic additives (such as organic dispersants) are mainly used to allow silicon and phosphorus to be evenly distributed in the silicon-phosphorus slurry.

[0071] In step 72, the drying temperature of the silicon-phosphorus slurry is 200-400°C (eg, 330°C) to evaporate most of the organic additives.

[0072] It should be noted that in step 72, the thickness of the dried silicon-phosphorus slurry 9 is at least 1 μm greater than the thickness of the anti-reflection film. This can effectively prevent the subsequently printed aluminum paste from burning through the N+ polysilicon layer 4, protect the passivation structure of the N+ polysilicon layer 4 from being damaged, improve the passivation effect, and reduce metal recombination.

[0073] In step 72 , the width of the dried silicon-phosphorus slurry 9 is preferably at least 80 μm greater than the width of the laser-cut notch 8 .

[0074] Step 73, locally print fine grid metal paste on the back of the dried silicon phosphorus paste 9, and dry it. The drying temperature is 200-400° C. (such as 350° C.). The structure of the silicon substrate 1 after step 73 is as follows: Figure 8 shown.

[0075] In step 73, the fine gate metal paste is aluminum paste or nickel paste, and the width of the dried fine gate metal paste 10 is smaller than the width of the dried silicon phosphorus paste 9. Preferably, the width of the dried fine gate metal paste 10 is at least 20 μm smaller than the width of the dried silicon phosphorus paste 9.

[0076] Step 74, after printing the front metal paste (such as silver paste) locally on the front side of the passivation anti-reflection film of the silicon substrate 1, the entire silicon substrate 1 is pre-sintered and sintered in sequence, and cooled, so that the silicon-phosphorus paste forms a eutectic layer 91 of phosphorus silicon and N+ polysilicon, a heavily phosphorus-doped microcrystalline silicon layer (the heavily phosphorus-doped microcrystalline silicon layer is also called N++ microcrystalline silicon layer 92) and a fine-gate metal silicon alloy 93 in the laser grooved area from top to bottom, and the main gate metal paste and the fine gate metal paste form the back electrode 11 together, and the front metal paste forms the front electrode 12. The photovoltaic cell structure after step 74 is as follows Fig. 9 shown.

[0077] In step 74, the fine gate metal silicon alloy 93 is an aluminum silicon alloy or a nickel silicon alloy. The pre-sintering temperature is 300-550°C, and the pre-sintering time is 8-12s (preferably 10s); the sintering temperature is 600-700°C, and the sintering time is less than 1s. During the above-mentioned pre-sintering and sintering, since the pre-sintering temperature is low and the sintering time is short, the temperature of the middle section of the silicon-phosphorus slurry rises slowly and does not reach the peak sintering temperature, a microcrystalline phase (i.e., a heavily phosphorus-doped microcrystalline silicon layer) will be formed, and electrons can be better conducted here.

[0078] It should be noted that the fine gate of the back electrode 11 is in ohmic contact with the N+ polysilicon layer 4 through the fine gate metal silicon alloy 93 (such as aluminum silicon alloy), the N++ microcrystalline silicon layer 92 and the eutectic layer 91 of phosphorus silicon and N+ polysilicon, and the main gate of the back electrode 11 is in ohmic contact with the N+ polysilicon layer 4. The front electrode 12 is in ohmic contact with the P+ emitter 2.

[0079] In a photovoltaic cell metallization method of the present embodiment, the width of the dried silicon-phosphorus slurry 9 is set to be larger than the width of the laser groove opening 8. The main reason is that after the laser selectively removes the anti-reflection film, the passivation performance of the laser groove area becomes poor. After the dried silicon-phosphorus slurry 9 is pre-sintered and sintered, it can achieve heavy phosphorus doping in the laser groove area to form an N++ microcrystalline silicon layer 92. The N++ microcrystalline silicon layer 92 can enhance the field passivation effect of the laser groove area.

[0080] In practice, the burn-through performance of aluminum paste or nickel paste is much stronger than that of silver paste. During the sintering process of aluminum paste (or nickel paste), a pinning effect is easily generated, resulting in the burn-through of the N+ polysilicon layer 4 and the tunnel oxide layer 3, resulting in a large battery leakage current, affecting the field passivation effect, and increasing metal recombination. Based on this, in this embodiment, the width of the dried fine gate metal paste 10 (aluminum paste or nickel paste) is narrower than the width of the dried silicon-phosphorus paste 9, and the thickness of the dried silicon-phosphorus paste 9 is at least 1 μm greater than the thickness of the anti-reflection film; this can effectively prevent the sintered fine gate metal paste (aluminum paste or nickel paste) from burning through the N+ polysilicon layer 4 and the tunnel oxide layer 3, protect the passivation structure such as the N+ polysilicon layer 4 and the tunnel oxide layer 3 from being damaged, improve the passivation effect, effectively prevent battery leakage current, and reduce metal recombination.

[0081] In the prior art, the thickness of the tunnel oxide layer 3 on the back of the silicon substrate 1 is usually 1-3 nm, and the tunnel oxide layer 3 forms chemical passivation by bonding with the dangling bonds of the silicon substrate 1. The thickness of the doped polysilicon layer (such as the N+ polysilicon layer 4) on the back of the tunnel oxide layer 3 is usually 90-110 nm, and the N+ polysilicon layer 4 forms an n+ field on the back of the tunnel oxide layer 3. When the thickness of the doped polysilicon layer such as the N+ polysilicon layer 4 is further reduced (that is, the N+ polysilicon layer 4 is thinner, for example, the thickness of the N+ polysilicon layer 4 is 50-60 nm), the thinner N+ polysilicon layer 4 can effectively reduce parasitic light absorption, and can also reduce production costs and improve production efficiency. However, the thinner N+ polysilicon layer 4 may also cause defects such as partial burn-through of the back passivation structure of the N+ polysilicon layer 4 and the tunnel oxide layer 3 during sintering of the aluminum paste or nickel paste, causing the burned-through aluminum paste (or nickel paste) to directly contact the silicon substrate 1 and destroy the passivation effect.

[0082] Based on this, in this embodiment, before printing aluminum paste (or nickel paste), phosphorus silicon paste is printed in the laser grooved area as a transition structure, so that the N+ polysilicon layer 4 can contact with the phosphorus silicon paste, and after printing the aluminum paste (or nickel paste), the aluminum paste (or nickel paste) can also contact with the phosphorus silicon paste, and then combined with the above-mentioned pre-sintering and sintering processes of this embodiment. In this way, (1) during sintering, the phosphorus silicon paste can greatly improve the safety of aluminum paste (or nickel paste) sintering, effectively prevent the passivation structure damage caused by aluminum paste (or nickel paste) burning through the N+ polysilicon layer 4, ensure the passivation effect, avoid battery leakage current, and reduce metal recombination. (2) Because the phosphorus silicon paste has a blocking effect on the burning through of aluminum paste (or nickel paste), the N+ polysilicon layer 4 can be further thinned (the N+ polysilicon layer 4 can be thinned to 50-60nm), thereby reducing the back parasitic light absorption, increasing the light utilization rate, and then increasing the short-circuit current, and improving the photoelectric conversion efficiency of the battery. (3) At the same time, the middle section of the sintered phosphorus silicon slurry can also enable the laser grooved area on the back of the N+ polysilicon layer 4 to be heavily doped with phosphorus, forming an N++ microcrystalline silicon layer 92, thereby improving the field passivation effect. (4) After sintering, the sintered phosphorus silicon slurry can form a phosphorus silicon and N+ polysilicon eutectic layer 91, an N++ microcrystalline silicon layer 92, and an aluminum silicon alloy (or a nickel silicon alloy) from top to bottom, so that electrons can be better conducted in the laser grooved area, thereby improving the electron transmission performance between the back electrode 11 (such as an aluminum electrode or a nickel electrode) and the N+ polysilicon layer 4, and effectively reducing the contact resistivity. (5) By widening the printing width of the dried silicon-phosphorus paste 9 (that is, making the width of the dried silicon-phosphorus paste 9 at least 80 μm larger than the width of the laser slot 8), and making the width of the dried fine-grid metal paste 10 at least 20 μm smaller than the width of the dried silicon-phosphorus paste 9; in this way, the printing width of the aluminum paste (or nickel paste) can be increased. The printing of large-line width aluminum paste (or nickel paste) can reduce line resistance loss, significantly improve the FF (fill factor) of the battery, and improve the efficiency of the battery cell. In addition, aluminum paste (or nickel paste) is cheaper than silver paste, so it can also reduce costs.

[0083] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present invention.

[0084] The technical solution provided by the present invention is introduced in detail above. Specific examples are used in this article to illustrate the principle and implementation mode of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation mode and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A photovoltaic cell metallization method, characterized in that: The steps include: S1. Prepare a silicon substrate, wherein a tunneling oxide layer, an N+ polysilicon layer and an anti-reflection film are sequentially provided on the surface of the silicon substrate; S2, performing laser selective etching on the anti-reflection film to form laser notches in the local area of ​​the anti-reflection film that partially expose the N+ polysilicon layer; S3, printing silicon-phosphorus slurry on the surface of the exposed N+ polysilicon layer, and drying, so that the dried silicon-phosphorus slurry covers the laser-cut notches; S4, locally printing a first metal paste on the surface of the dried silicon-phosphorus paste, and drying it; the first metal paste is aluminum paste or nickel paste; S5. The entire silicon substrate is pre-sintered and sintered in sequence, and cooled, so that the sintered first metal slurry forms a first electrode, and the sintered silicon-phosphorus slurry forms a eutectic layer of phosphorus silicon and N+ polycrystalline silicon, an N++ microcrystalline silicon layer and a first metal silicon alloy between the N+ polycrystalline silicon layer and the first electrode in sequence; the first metal silicon alloy is an aluminum silicon alloy or a nickel silicon alloy, and the first metal silicon alloy contacts the first electrode.

2. A photovoltaic cell metallization method according to claim 1, characterized in that: In step S3, the silicon-phosphorus slurry is a mixture of silicon element, glass powder, phosphorus element, and organic additive in a mass ratio of 11-16:2-7:1:1; the organic additive is an organic dispersant or a thixotropic agent; The thickness of the dried silicon-phosphorus slurry is greater than the thickness of the anti-reflection film, and the width of the dried silicon-phosphorus slurry is greater than the width of the laser notch; the drying temperature of the silicon-phosphorus slurry is 200-400°C.

3. A photovoltaic cell metallization method according to claim 2, characterized in that: The thickness of the dried silicon-phosphorus slurry is at least 1 μm greater than the thickness of the anti-reflection film; the width of the dried silicon-phosphorus slurry is at least 80 μm greater than the width of the laser-grooved opening.

4. A photovoltaic cell metallization method according to claim 1, characterized in that: In step S4, the width of the first metal slurry after drying is smaller than the width of the silicon-phosphorus slurry after drying; The drying temperature of the first metal slurry is 200-400°C.

5. A photovoltaic cell metallization method according to claim 4, characterized in that: The width of the first metal paste after drying is at least 20 μm smaller than the width of the silicon-phosphorus paste after drying.

6. A photovoltaic cell metallization method according to claim 1, characterized in that: In step S5, the pre-sintering temperature is 300-550°C, and the pre-sintering time is 8-12s; the sintering temperature is 600-700°C, and the sintering time is less than 1s.

7. A photovoltaic cell metallization method according to any one of claims 1 to 6, characterized in that: In step S1, the thickness of the N+ polysilicon layer is 50-60 nm; In step S3, before printing the silicon-phosphorus slurry, the step further includes: locally printing a second metal slurry on the surface of the anti-reflection film and drying it; The first metal paste is a fine gate metal paste, and the second metal paste is a main gate metal paste.

8. A method for preparing a photovoltaic cell, characterized in that: The method comprises the following preparation steps: Step 1: Prepare a P+ emitter on the front side of the silicon substrate; Step 2: sequentially preparing a tunnel oxide layer and an N+ polysilicon layer on the back side of the silicon substrate; Step 3: prepare a passivation anti-reflection film on the front side of the P+ emitter, and prepare an anti-reflection film on the back side of the N+ polysilicon layer; Step 4: metallizing the silicon substrate treated in step 3 using a photovoltaic cell metallization method as described in any one of claims 1 to 7; In step S5, before pre-sintering, the method further includes: printing a front metal paste locally on the front surface of the silicon substrate.

9. A photovoltaic cell, characterized in that: It is prepared by the method for preparing a photovoltaic cell as described in claim 8.

10. A photovoltaic module, characterized in that: It comprises the photovoltaic cell as claimed in claim 9.